A cup four to five times the volume of the silicone it holds, and a foam that can still climb to seven times that volume: the two figures sit on the same Renishaw data sheet for Vacusil 2000, and they describe a moment of about two or three minutes in which the mix looks as if it will leave the container. Then the foam collapses, the surface settles, and the silicone that goes over the master is ready. A resin component in the casting chamber goes through a quieter version of the same event, ten minutes long, before anyone mixes anything.
Degassing is the one operation in vacuum casting that the process is named after, and it is also the one a buyer never sees in a photograph of a finished part. What it leaves behind can be seen. A silvery pinhole on a face, a void under an overhang, a cloudy wall in a clear lens and a surface that looks like fine foam each trace to air or gas that was in the mix, or entered it afterward, and each has a different cure.
Why Silicone and Resin Are Degassed Under Vacuum
Mixing puts air into any liquid. Stirring two viscous components together folds the surface into the bulk, and a general guide from the mold supplier ArtMolds puts the air picked up by mixing at 5 % to 20 % of the volume, calling it the primary cause of bubbles in cast parts. A bubble that small does not rise out of a thick liquid on its own, because the buoyant force is tiny compared with the drag of the viscous material around it.
Vacuum changes the sum. With the surrounding pressure lowered, each bubble expands, gains buoyancy and travels to the surface, where it breaks. Polytek, a maker of casting rubbers and resins, describes the effect plainly: small bubbles lack the buoyancy to rise through thick material, but the vacuum expands them until they float up and pop. The same page advises degassing silicones above roughly 20,000 cps. Vacusil 2000 mixes to 45,000 mPa·s at 23 °C (one mPa·s equals one cps), so it sits well above that line, and its sheet asks for a vacuum step as a matter of course.
Two different things are removed, and keeping them apart helps later in this piece. Air that was whipped in during mixing is removed by vacuum. Gas that the chemistry itself produces, which is carbon dioxide from water meeting isocyanate, is not removed by vacuum once it has formed. The first is a handling problem, the second a storage problem.
Vacuum removes air that was mixed in, and it cannot remove carbon dioxide that the resin has already made from moisture.
Where Degassing Sits in the Cycle
Degassing happens at four points in a tool’s life. The silicone is degassed once in its cup and once again after it is poured over the master. For every copy, each resin component is degassed in its own cup, and the mixed resin is poured in the chamber before the air is let back in. Each of these has its own time limit, and each limit comes from a different clock: the silicone’s pot life of 90 minutes at 23 °C for the tool, the resin’s pot life of minutes for the copy.
What the Vacuum Level Does to a Bubble
A bubble in a liquid follows the gas law at constant temperature closely enough for a buyer’s purpose: its volume varies inversely with the pressure on it. At a gauge vacuum of 29 inHg (about 982 mbar below atmosphere) leaves about 0.92 inHg absolute, which is about 31 mbar, and a bubble that was 1 mm³ at sea level pressure then wants about 32 mm³. The table gives the same arithmetic for the gauge readings that casting rooms quote. It assumes a standard atmosphere of 29.92 inHg (1,013 mbar) and ignores surface tension and the liquid’s own head, so it states the ceiling, not a measurement.
| Gauge vacuum | Below atmosphere | Absolute pressure | Bubble volume against sea-level size |
|---|---|---|---|
| 20 inHg | 677 mbar | 336 mbar (9.9 inHg) | 3.0 times |
| 25 inHg | 847 mbar | 167 mbar (4.9 inHg) | 6.1 times |
| 28 inHg | 948 mbar | 65 mbar (1.9 inHg) | 15.6 times |
| 29 inHg | 982 mbar | 31 mbar (0.9 inHg) | 32.5 times |
| 29.5 inHg | 999 mbar | 14 mbar (0.4 inHg) | 71 times |
Each half step near full vacuum buys far more expansion than a step in the middle of the range. Moving from 20 to 25 inHg doubles the factor, and moving from 29 to 29.5 inHg doubles it again. The maker sheets in this piece name a time at vacuum and never a pressure target, which leaves the gauge to the machine. Polytek names 29 to 30 inHg as the range at which a mix begins to foam.
A gauge reads against the local atmosphere. Above sea level the room starts from a lower pressure, so the absolute figures in the table belong to a sea-level room only.
The expansion factor doubles between 29 and 29.5 inHg, which is why the last fraction of vacuum is where a mix foams hardest.
Degassing the Mold Silicone Twice
The silicone rubber that becomes the tool is the first thing degassed, and the maker’s procedure is specific. Renishaw’s Vacusil 2000 sheet asks for a mixing container four to five times larger than the volume of silicone, a weighed 100:10 mix scraped from the sides and bottom so no unmixed pockets remain, and a vacuum run of around 2 to 3 minutes. The sheet adds that the silicone can expand up to 7 times its original volume during degassing, which is why the container is sized as it is.
A cup that holds only four to five times the volume of the liquid can cope with a sevenfold rise because the foam is not a stable column. Polytek’s advice on the same behavior is that once the rubber has risen and fallen it will not rise again, and that holding the material under vacuum for 2 to 3 minutes after the foam falls clears what is left. The Renishaw figure of 2 to 3 minutes covers the whole run, so the two sources differ on whether the clock starts at pump-on or at collapse. A room that follows one maker’s silicone adopts that maker’s reading.
The Pour and the Second Degas
After degassing, the silicone goes into the mold frame as a slow, steady stream so it flows around and over the master. Air still gets trapped, mostly under overhangs, in recesses facing down and against the master’s flat faces. The Vacusil sheet therefore recommends secondary degassing once the pour is complete, to remove voids around or under the model, and it states that the whole degassing process has to be carried out well within the working time of the mixed silicone. With a pot life of 90 minutes at 23 °C, the first degas of 2 to 3 minutes, the pour, and the second degas fit together with time to spare, and a cold room stretches the margin further.
ArtMolds adds the placement side of the same fight: vents go at every high point where air collects, and rigid wires pulled out after cure leave the channels. In vacuum casting the same job is done by the gate and vent rods that become channels in the cut tool.
The sequence for one silicone block, in the order the sheet gives it:
- Weigh silicone and catalyst 100:10 into a clean, dry cup four to five times the silicone’s volume.
- Mix, scraping the sides and bottom, then pull vacuum for about 2 to 3 minutes while the foam rises and falls.
- Pour in a slow, steady stream so the silicone flows around and over the master.
- Pull a second vacuum to clear voids under the master, well inside the 90 minute pot life.
Reading the Silicone Block After Cure
A void in the cured block is a hole in the finished tool, and the face of the copy shows it as a raised bead or lump. Voids against the master’s surface are the dangerous ones, since they sit exactly where a copy takes its shape. A cloudy or sticky skin on the silicone that never reached full cure is a different fault, cure inhibition from a contaminant, and the sheet’s remedy for that is a patch test and not more vacuum.
| Material | What is degassed | Time and condition | Maker and sheet |
|---|---|---|---|
| Vacusil 2000 silicone | mixed silicone, cup 4 to 5 times its volume | about 2 to 3 min; expands up to 7 times; second degas after pouring, inside the pot life | Renishaw, Vacusil 2000, issued 10.2017 |
| SikaBiresin PX523 | polyol and isocyanate, each alone | 10 min each; then mixed in vacuum 2 to 3 min | Sika, PX523 data sheet, version 01.01 |
| SikaBiresin PX331 | both components, each alone | 10 min each; then mixed in vacuum at least 1 min | Sika, PX331 data sheet, version 01.01 |
| Renishaw 6230 and 8263 | both cans in the chamber | wait 10 min after maximum vacuum before mixing; mixing time 60 s | Renishaw data sheets, issued 09.2015 and 05.2015 |
| Renishaw 8020-2 | both cans in the chamber | wait 10 min after maximum vacuum; mixing 45 s to 60 s | Renishaw, issued 04.2018 |
| Sika PX 223 HT | each part, before use | degas each part; mix about 45 s | Sika, TDS version 01, 2021 |
Degassing Each Resin Component Alone
The two resin components are never degassed together. Chemistry sets the reason: the moment polyol and isocyanate meet, the pot life starts, and a mix that has to be degassed afterward is racing its own gel. Sika’s sheets therefore ask for each component to be evacuated separately for 10 minutes, in its own cup, before anything is combined. Renishaw’s resin sheets say the same in different words: start the vacuum pump, switch on the mixer motor, and wait 10 minutes after reaching maximum vacuum level before mixing.
The mixing then happens inside the chamber, at a short fixed time. Mixing in vacuum runs 2 to 3 minutes on the PX523 sheet, at least 1 minute on PX331, 60 seconds on Renishaw 6230 and 8263 and 45 to 60 seconds on 8020-2. Those times matter because the pot life behind them is short. PX331 gels in 6 minutes on a 200 g mass at 23 °C by Sika’s gel timer method, Renishaw 6230 gives 6 minutes on 100 g at 25 °C and 3 minutes 40 seconds at 35 °C, and PX523 at 20 minutes on 162 g at 23 °C is the longest of the set.
Cup Loss and the Order of Pouring
The upper cup never empties entirely, and both Sika and Renishaw tell the operator to weigh with that loss in mind. Renishaw defines it as the amount of resin left in cup A after tipping. The Sika sheets place the polyol in the upper cup for PX523 and the isocyanate in the upper cup for PX205 and PX331, so the cup that holds the residue differs from grade to grade, and the weighing allowance sits on whichever component is in the upper cup.
Temperature Changes How Fast Bubbles Leave
A warmer component is thinner and degasses faster, and it also gels sooner. Renishaw has the cans preheated at 70 °C for 2 hours and then held in a 40 °C oven to stabilize before use, while the Sika grades on file ask for 18 °C to 25 °C. The Renishaw sheets add that the exact resin temperature and the exact mold temperature are important, which fits the 3 minutes 40 seconds against 6 minutes pot life difference between 35 °C and 25 °C for the same resin.
A resin that foams in the cup before mixing has told the operator something about the can, not about the pump.
Moisture Bubbles That Vacuum Does Not Remove
Polyurethanes are made from polyols and isocyanates, and ResinLab’s technical bulletin states that both are hygroscopic and absorb moisture from the atmosphere. When an isocyanate meets water it forms carbon dioxide and amines, and the amines react with more isocyanate to form polyurea linkages. The gas appears in the cured material as bubbles and, with enough water, as foam. That bulletin also notes that aliphatic isocyanates are less reactive with water than aromatic ones, so the choice of isocyanate changes how sensitive a grade is.
Maker sheets for casting resins treat this as a daily handling point. Sika asks that both containers be closed tightly immediately after use to prevent moisture ingress and that an opened product be used as soon as possible. Renishaw states that all components are sensitive to humidity and has opened cans stored in a 40 °C oven with caps on. For pigmented parts, Sika’s PX331 sheet asks that pigments be free of moisture before application, which puts the color paste on the same list as the cans.
What a Moisture Fault Looks Like
ResinLab lists signs in the container: an isocyanate may look cloudy, may carry solid material at the bottom or form a solid layer on top, whereas a contaminated polyol generally looks the same as a good one. After the pour the signs are in the part, as fine bubbles scattered through the material, often in the thicker sections where the gas had time to gather. Those bubbles are gas, and degassing the cup again does nothing for a can that has already reacted.
Crystallization is a separate fault with a separate cure. Sika’s sheets say that crystals in a component after prolonged cold storage can be reversed by heating the affected component to a maximum of 70 °C until they have gone, then cooling it to processing temperature. Renishaw gives 70 °C for 2 hours, then 40 °C to stabilize, and for 8020-2 2 to 4 hours at 70 °C followed by stirring.
A component that has taken up water will stay a source of bubbles however long it sits under vacuum, so the fix is a fresh can or a sealed one.
Letting the Air Back In and Reading the Part
Once the mixed resin is in the tool, the chamber has to be vented before the pot life ends. Renishaw’s procedure says to pour the mixed resin into the silicone mold and leak the vacuum chamber before the end of the pot life. The air coming back pushes the resin into the tool’s thin sections and compresses any bubble still sitting in the cavity, and it has to happen while the resin can still flow.
Faults that follow from the degassing step read differently on the part, and the next table sorts them by what a buyer or an inspector sees first.
| What is seen | Likely cause | What to check |
|---|---|---|
| a scatter of fine bubbles through the whole part | moisture in a can or in pigment | can history, caps, pigment dryness, crystallization treatment |
| a few large voids high in the cavity | air trapped by a poor vent or a vent rod set low | vent rod placement, pour angle, second degas of the silicone |
| bubble or lump on the face of a copy, same place every time | a void in the silicone against the master | the cut tool at that spot, since the same void repeats on every copy |
| short, unfilled corner | resin thickening before the air returned, or a cold tool | time from pour to venting, tool at 70 °C, pot life at component temperature |
| cloudy skin or tacky surface on the silicone | cure inhibition, not trapped air | patch test of master coating and tapes |
| foam climbing the wall of the resin cup | cup too small or component wet | cup volume, can storage |
Checks the Operator Can Write Into a Batch Record
Four records settle most degassing disputes, and a buyer can ask for them in the batch documentation:
- the time at maximum vacuum for each component before mixing, in minutes,
- the resin and mold temperatures at the pour, in °C,
- the time from the start of mixing to the leak, set against the pot life on the sheet,
- the condition of the opened cans: how long open, how stored, and whether caps were on.
None of the four needs a special instrument. A clock, a thermometer and a notebook cover them.
Why a Clear Grade Shows It First
A clear part shows every bubble, since a bubble in a lens is a lens. PX522, a clear grade for parts up to 10 mm thick, carries a note on its sheet to cast it in a new mold without casting resin previously inside, which treats the tool’s own history as a possible source of trouble. Clear grades leave no place for a bubble to hide, so they are the grades for which a buyer has the clearest reason to ask for a degassing record.
What Degassing Adds to the Calendar
The last point is a calendar one. Each pour costs about 10 minutes of waiting at vacuum for each component on the grades above, and the clear grades that run 20 minutes of pot life leave the most room to do it properly. A batch of 100 parts from tools that give 30 to 50 copies each needs at least 100 degassing cycles on the resin side, and each cycle repeats the waiting, so degassing time scales with the number of copies and not with the number of tools. That is the fixed cost the operation sets under every quantity. For parts that need more than a few dozen copies per color and grade, a buyer asks whether a low-volume vacuum casting schedule built around those cycle counts still fits, or whether the quantity belongs in bridge production.
Sources and Further Reading
- Renishaw, Data sheet: Vacusil 2000 silicone rubber, issued 10.2017
- Renishaw, Data sheet: vacuum casting resin 8263, issued 05.2015
- Renishaw, Data sheet: vacuum casting resin 6230, issued 09.2015
- Renishaw, Data sheet: vacuum casting resin 8020-2, issued 04.2018
- Sika, SikaBiresin PX523, product data sheet, version 01.01
- Sika, SikaBiresin PX331, PX205 and PX522 product data sheets, version 01.01 (08-2026), industry.sika.com
- Sika, PX 223 HT, technical data sheet, version 01, 2021
- ResinLab, Moisture Contamination of Polyurethanes, technical bulletin, 2021
- Polytek Development Corp., What is vacuuming and why should I do it
- ArtMolds, Air bubbles and air traps