Data SheetPolyurethaneBatch

ISO 179 and ISO 180 Impact Strength on Cast Resin Data Sheets

Impact values on cast resin sheets are comparisons tied to method, notch, specimen and cure, so a part's toughness is set by tests on batch bars or the part.

Small notched cast polyurethane impact test bars in black and white, two broken clean at the notch and one bent but whole.

One page of Sika’s North American sheet for PX 223 HT prints two impact results for the same cured resin. Notched, to ASTM D256, the figure is 3 ft·lb/in² (6 kJ/m²). Charpy, to ISO 179, the figure is “greater than 29 ft·lb/in² (greater than 60 kJ/m²)”, with a footnote explaining that the samples did not break and the value is the impact energy with no fracture.

A tenfold gap on one material is not an error. It is what happens when two methods, a notch and a different specimen meet the same resin. Impact strength is the property on a polyurethane casting material sheet that is easiest to misread, because it looks like one number and is in fact a test configuration expressed as energy per area. Read through the two ISO standards that most sheets cite, it becomes a useful comparison and a poor design value.

What ISO 179 and ISO 180 Measure on a Cast Resin

Both standards measure how much energy a pendulum hammer loses breaking a small bar of plastic at a high strain rate. ZwickRoell, a maker of the testing machines, describes the principle in its pages on both methods: a hammer of specified energy and drop height strikes the specimen, does not swing back to its starting height, and the height difference is taken as the energy absorbed. The result is divided by the specimen’s cross-section and printed in kJ/m².

The two differ in how the bar is held. In ISO 179 (Charpy), the bar lies on two supports and the hammer strikes it in the middle, a three-point flexure fixture. Under ISO 180 (Izod), the bar is gripped at one end and struck as a cantilever; ZwickRoell gives its specimen as 10 × 4 × 80 mm (0.39 × 0.16 × 3.15 in). Both can be run on notched or unnotched bars, and ZwickRoell notes that the two methods deliver similar conclusions about a material’s impact strength.

The published scopes say what the results are for. As published by the Estonian standards body, the ISO 180 scope covers rigid thermosetting molding materials among others and states that the method estimates brittleness or toughness within the limitations of its test conditions. ISO 179-2’s scope adds that the impact behavior of finished products cannot be predicted directly from the test.

ISO 179 and ISO 180 report the energy a pendulum spends breaking a standard bar, per unit of cross-section. They compare materials under identical conditions; they do not predict how a cast part will survive a drop.

The Impact Methods a Cast Resin Sheet May Cite

Five method names appear on the sheets and pages on file, and ZwickRoell names a sixth, ASTM D6110, as the ASTM counterpart of the Charpy test. Each is a separate configuration, and the table places them side by side as their own documents describe them.

Table 1. Impact methods named on cast resin data sheets, and how each is set up, from the standards bodies’ scopes and the testing machine maker’s pages
Method Support of the bar What the result is Notes from the opened documents
ISO 179-1 (Charpy, non-instrumented) on two supports, struck in the middle energy per cross-section, kJ/m² preferred by ISO 10350-1 for single-point data, ideally unnotched with edgewise impact (code 1eU); notched bars if the unnotched bar does not break
ISO 179-2 (Charpy, instrumented) as ISO 179-1 force-deflection diagram and energies derived from it detects break type and operating mistakes; results comparable only for identical preparation and test conditions
ISO 180 (Izod) gripped at one end energy per cross-section, kJ/m² 10 × 4 × 80 mm bar; edgewise impact common, flatwise less common; notched or unnotched
ASTM D256 (Izod) gripped at one end energy per unit width or per area under the notch milled notch; methods A, C, D and E; method E strikes the reversed notch

ASTM figures need care in reading. Its scope states that results are reported as energy absorbed per unit of specimen width (J/m or ft·lbf/in) or per unit of cross-sectional area under the notch. Sika’s US sheets print D256 in ft·lb/in² with kJ/m² beside it, the area form. A buyer who meets a D256 value in J/m has a different quantity, and cannot set it beside a kJ/m² figure without conversion through the specimen dimensions.

ZwickRoell adds that ISO 180’s method is based on ASTM D256 but uses different specimen dimensions. The same resin, tested by the two, gives two numbers.

How Cast Resin Makers Print Their Impact Values

The sheets on file use every one of the configurations above, and they print them in different shapes: a plain number, a “no break”, a “greater than”, or a blank.

Table 2. Impact values on cast polyurethane sheets, with the method and the cure or condition each sheet states
Grade Method printed Value Cure or condition stated
Sika PX331 ISO 179 (CQP038-2) 26 kJ/m² (12.4 ft·lb/in²) post-cure 70 °C (158 °F) 1 h, then 80 °C (176 °F) 16 h
Sika PX522 with PX521 ISO 179 (CQP038-2) 48 kJ/m² (22.8 ft·lb/in²) post-cure 80 °C (176 °F) 4 h, then 100 °C (212 °F) 16 h
Sika PX523 ISO 179 (CQP038-2) 42 kJ/m² (20.0 ft·lb/in²) post-cure 100 °C (212 °F) 16 h
Sika UR390 (elastomeric) ISO 179 (CQP038-2) no break cure 70 °C (158 °F) 16 h
Sika PX 223 HT ISO 179/2D:1994 above 60 kJ/m² (above 29 ft·lb/in²), did not break post-cure 70 °C 1 h, 100 °C 1 h, 110 °C 12 h (158, 212, 230 °F)
Sika PX 223 HT ASTM D256-05, notched and unnotched 6 kJ/m² (3 ft·lb/in²) notched; above 16 kJ/m² (above 8 ft·lb/in²) unnotched, did not break as above
Sika PX 1000 ASTM D256-05, notched 6 kJ/m² (2.9 ft·lb/in²) post-cure 12 h at 70 °C (158 °F)
Renishaw 8045 to 8045-3 ISO 180 16, 16, 19, 21 kJ/m² (7.6, 7.6, 9.0, 10.0 ft·lb/in²) cure 60 min at 60 °C (140 °F)
Renishaw 8040 ISO 180 (Izod) 15 kJ/m² (7.1 ft·lb/in²) no post-cure
Renishaw 8060-2 ISO 180 (Izod) 15 kJ/m² (7.1 ft·lb/in²) post-cure chosen for heat deflection

Four reading rules come out of the table.

  1. Look for the notch. The Sika German sheets and the Renishaw sheets do not say whether their bars were notched. PX 223 HT shows how much the answer matters: 6 kJ/m² notched against more than 16 kJ/m² unnotched on the same resin and test.
  2. Treat “no break” and “greater than” as limits. They say the bar survived the hammer used, not how much energy the material can absorb. UR390’s “no break” and PX 223 HT’s “above 60” cannot be ranked against each other.
  3. Compare Charpy with Charpy and Izod with Izod. A Renishaw Izod figure of 15 to 21 kJ/m² beside a Sika Charpy figure of 26 to 48 kJ/m² is two methods, not a ranking of two makers’ resins.
  4. Read the cure. Every value in the table follows a stated cure, and the cures differ by hours and tens of degrees.

An impact value on a cast resin sheet carries five pieces of information: method, notch, specimen, cure and the number itself. Without the first four, the fifth ranks nothing.

Why Notched and Unnotched Results Differ So Much

The ASTM D256 scope explains the role of the notch. An Izod specimen’s notch concentrates stress, minimizes plastic deformation and directs the fracture to the part of the specimen behind the notch, which reduces scatter. It also, in the scope’s words, increases the probability of a brittle rather than a ductile fracture. Because plastics respond differently to a given notch, the standard offers method D, comparing bars with different notch radii, as a measure of notch sensitivity.

For a cast part, the notch is a design question. A sharp inside corner, a molded-in thread root or a thin rib meeting a wall acts as a notch. Even a material whose unnotched bar does not break can still crack at such a corner, and the notched figure is the closer guide to that behavior.

The D256 page lists what else moves the result, and the list reads like a description of vacuum casting variables: the method of fabrication, including processing technology, molding conditions, mold design and thermal treatments, then the method, speed, design and quality of the notching. A cast bar and a machined bar of the same resin are not guaranteed to agree.

The same page records a documented discrepancy between manual and digital impact testers, mainly with thermoset materials of impact values under 54 J/m (1 ft·lbf/in). It also requires its method C, with a correction for the energy spent throwing the broken piece, for materials below 27 J/m (0.5 ft·lbf/in). Brittle cast thermosets sit near those thresholds, and the lab’s method choice is part of the result.

How the Test Itself Is Controlled

A buyer does not run pendulum tests, but knowing how labs keep them comparable explains what a supplier can certify. ZwickRoell describes the controls on both its pages.

Machine verification. Pendulum testers are specified in ISO 13802, whose scope, as published by the Estonian standards body, covers the frequency and methods for verifying pendulum machines used for Charpy, Izod and tensile impact tests.

Hammer selection. Each hammer is used between 10 % and 80 % of its initial potential energy. Where several hammers qualify, the one with the greatest energy is used, which keeps the loss of speed during impact small.

Losses. All energy losses are attributed to the specimen, so friction in the bearings and air resistance are measured and corrected during calibration, and the tester stands on a stiff, vibration-free base.

Conditioning. Izod tests to ISO 180 are normally run after conditioning in a normal climate of 23 °C (73 °F) and 50 % relative humidity to ISO 291. Charpy tests are run in normal climate or at low temperature.

Low temperature. ZwickRoell notes that Charpy suits low-temperature work better, because the supports sit further from the notch and the specimen loses less cold while it is moved from the cooling device into the tester.

The ISO 179-2 scope adds what instrumentation brings: a force-deflection record, automatic detection of the break type, and detection of mistakes such as a specimen not resting against its supports. It closes with the caution that results compare only when specimen preparation and test conditions are the same.

Impact Against Stiffness Across One Maker’s Range

Sika’s tooling and composites brochure prints an impact column for its whole vacuum casting range, as approximate values beside an E-modulus. Checked against the grades’ own sheets, that E-modulus equals the flexural modulus to ISO 178: 3,700 MPa for PX331, 2,400 for PX522, 2,100 for PX523. Where a grade also has its own sheet, the brochure’s impact figure matches the sheet’s ISO 179 value: 48 kJ/m² for PX522, 42 for PX523, 26 for PX331. Read across the range, the column shows the trade every rigid cast grade makes.

Table 3. Impact strength against flexural stiffness for Sika’s rigid vacuum casting grades, brochure approximate values
Grade Brochure description E-modulus (flexural) Impact strength
PX221 properties similar to HIPS 2,100 MPa (305,000 psi) 71 kJ/m² (33.8 ft·lb/in²)
PX226 similar to filled ABS 2,500 MPa (363,000 psi) 70 kJ/m² (33.3 ft·lb/in²)
PX245 similar to polyoxymethylene and polyamide, stiffest 4,500 MPa (653,000 psi) 30 kJ/m² (14.3 ft·lb/in²)
PX280 ABS type, good mechanical properties 2,800 MPa (406,000 psi) 25 kJ/m² (11.9 ft·lb/in²)
PX331 fire-classified, UL 94 V0 at 3 mm 3,700 MPa (537,000 psi) 26 kJ/m² (12.4 ft·lb/in²)
PX235 HT thermal resistance up to 190 °C (374 °F) 2,500 MPa (363,000 psi) 75 kJ/m² (35.7 ft·lb/in²)

The stiffest grade, PX245, prints less than half the impact energy of the HIPS-like PX221. No single grade is both the stiffest and the toughest, which is why a buyer reads the two columns together.

The table also carries a caution about labels. Its E-modulus of 3,700 MPa (537,000 psi) for PX331 is the sheet’s flexural modulus; the same sheet prints a tensile modulus of 4,500 MPa (653,000 psi). A brochure column headed E-modulus is therefore not compared with tensile values, and only the product sheet, with its method and cure, is the document to quote.

What ISO 179 and ISO 180 Leave Open for a Cast Part

The scopes are plain about the limits. According to the ISO 180 scope, tests on specimens of different dimensions, with different notches or prepared under different conditions may produce results that are not comparable, and that the method is not intended as a source of data for design calculations. Information on typical behavior, it adds, comes from testing at different temperatures, notch radii and thicknesses. The ISO 179-2 scope repeats that finished-product behavior cannot be predicted directly.

For a vacuum cast part, that leaves these questions to the buyer and the caster:

  • The geometry of the part. Wall thickness, corner radii and inserts change how the part takes a blow. No bar result covers them.
  • The temperature of use. Sheets print room-temperature values. A part that sees cold service is tested cold; Charpy is the method that suits it.
  • The cure of the delivered part. Table 2’s values follow post-cures of up to 20 hours. A part delivered after a shorter cure is not the tested material.
  • The direction of the blow. ISO 180 distinguishes edgewise and flatwise impact, and the sheets on file do not say which they used.

The ZwickRoell pages also list, among the uses of both tests, tolerance monitoring in goods-in checks and testing finished parts from machined specimens. Those are the two ways a buyer can turn the method into an acceptance check.

The impact standards say outright that their numbers are for comparison and quality control, not design. A cast part’s toughness is shown by testing the part, or bars machined from it, at the temperature it will see.

Specifying Impact Strength for Vacuum Cast Parts

An order or drawing that calls for impact strength on cast parts is clear when it fixes the variables the sheets leave loose.

  1. Name one method. ISO 179-1 Charpy or ISO 180 Izod for a European chain of supply, ASTM D256 where a US customer requires it, and not a mixture.
  2. State notched or unnotched, and for a notched test the notch type the standard defines.
  3. State the specimen. A cast bar poured with the batch in the same grade and cure, or a bar machined from a cast plate, which the ISO 180 scope allows.
  4. State the conditioning and temperature, 23 °C (73 °F) and 50 % relative humidity unless the part works colder or warmer.
  5. State the result form. A minimum in kJ/m², and how “no break” results are recorded.
  6. Tie it to the batch. First article only, or bars with every batch or resin lot.

With those six points, a figure such as 26 kJ/m² on PX331 or 16 kJ/m² on 8045 becomes a check the casting room can pass or fail. For runs of tens to hundreds of cast parts in a stated grade and cure, the check sits naturally inside low-volume vacuum casting, and the same bars, poured with each batch, carry the requirement through bridge production until the molded part takes over.

Sources and Further Reading

Send the Drawing of Your Cast Part

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Vacuum Casting chosen.

Request a Quote