An SLA master measured Ra 4.075 µm (160 µin). Three urethane parts cast from its silicone mold measured Ra 3.788, 3.576 and 3.686 µm (149, 141 and 145 µin). An FDM master of the same battery cover, Ra 22.075 µm (869 µin), gave parts at about Ra 21.7 µm (853 µin). The numbers come from a 2020 study at Universiti Teknologi Malaysia, and they say most of what a buyer needs to know about vacuum casting surface finish in one line: the cast part carries the master’s roughness, slightly smoothed, and almost nothing the casting room does afterward changes that by much.
The rest of this piece is about the “slightly” and the “almost”. Two published studies measured both masters and cast parts under stated stylus conditions, and the makers of masters, silicones and resins add what moves the surface between them.
How Closely a Vacuum Cast Surface Follows Its Master
A vacuum cast part’s surface roughness is set by its master within about a tenth of the master’s value, in the two studies on file. In the 2020 study by Mustafa and co-authors, parts cast from FDM, SLA and multi jet fusion (MJF) masters all came out smoother than the master, by 1.84 %, 9.62 % and 6.09 % respectively. The authors attribute the slight decrease to the properties of the materials used.
| Master | Master Ra | Cast part Ra | Change | Study |
|---|---|---|---|---|
| FDM, ABS | 22.075 µm (869 µin) | 21.631 to 21.718 µm (852 to 855 µin), mean 21.668 µm | 1.84 % lower | Mustafa et al., 2020 |
| MJF, polyamide | 14.548 µm (573 µin) | 13.501 to 13.940 µm (532 to 549 µin), mean 13.663 µm | 6.09 % lower | Mustafa et al., 2020 |
| SLA, white resin | 4.075 µm (160 µin) | 3.576 to 3.788 µm (141 to 149 µin), mean 3.683 µm | 9.62 % lower | Mustafa et al., 2020 |
| Silicone mold cavity, from an FDM ABS master smoothed in acetone vapor | 0.340 µm (13.4 µin), cavity average | 0.3 to 1.7 µm (12 to 67 µin) across 18 runs; 0.338 and 0.342 µm (13.3 and 13.5 µin) at the best settings | best runs equal to the cavity | Singh, Singh and Singh, 2017 |
Two observations matter more than the percentages. First, the ranking of masters carried straight through to the parts: FDM roughest, MJF in between, SLA smoothest. No casting setting in either study turned a rough master into a smooth part. Second, the spread among castings from one master was small, a few tenths of a micrometer on the SLA master’s parts, which is what a buyer sees as batch consistency.
The 2017 study by Singh, Singh and Singh shows the other end of the scale. Its masters were printed by FDM and then smoothed in acetone vapor for five cycles of 6 s each; the silicone mold cavity measured Ra 0.340 µm (13.4 µin), and the best castings matched it. Mustafa’s paper cites two earlier studies with vapor-smoothed masters whose castings measured Ra 0.319 to 0.667 µm and 0.455 to 0.593 µm (12.6 to 26.3 and 17.9 to 23.3 µin).
A vacuum cast surface is the master’s surface, copied. In the studies on file, parts came out 2 to 10 % smoother than their masters and kept the masters’ ranking, so the finish of a cast batch is chosen when the master is finished.
Why the Master Sets the Finish
Every guide on file says the same thing in its own way. Loughborough University’s vacuum casting guide states that the mold replicates the master extremely faithfully, so the surface finish and accuracy of the master have to be what is required of the molding.
The 2004 dissertation by F. C. Aggenbacht at the Central University of Technology, Free State, adds that deficiencies in the master’s surface will be reproduced in the cast part, and that the master should be as smooth as possible and sealed.
Renishaw’s vacuum casting brochure describes the cavity as perfectly replicating the master. The silicones that do the copying are chosen to keep that promise. Sika lists high surface quality, even for clear parts, among the properties of its SI291 silicone, and the Mustafa study used an addition-cure silicone because, in its words, addition-cure rubber shows virtually no shrinkage compared with condensation-cure rubber.
The same chain explains clear parts, the most demanding case. In the Aggenbacht dissertation, the master’s surface finish is noted as influencing the transparency of a cast clear part. Polytek’s bulletin for its clear Poly-Optic resins asks for highly polished masters to create molds of excellent surface quality, and warns that condensation-cure silicones are not recommended for them, because residual alcohol can inhibit cure or produce hazy castings. The finish of a cast batch is therefore decided at the printer or the mill: a 3D printed master carries its layer lines into the silicone unless they are sanded out first.
Surface Roughness of SLA, FDM, MJF and CNC Masters
The master’s process sets the starting roughness, and the studies give figures for three printing processes. In Mustafa’s battery cover, the as-built masters measured Ra 4.075 µm (160 µin) for SLA, 14.548 µm (573 µin) for MJF and 22.075 µm (869 µin) for FDM. The same paper reports the SLA master closest to the CAD model dimensionally as well.
A stereolithography master is not one surface. One 1997 paper by Ciba Specialty Chemicals and 3D Systems, presented at the University of Texas Solid Freeform Fabrication Symposium, explains that sidewall roughness on an SL part depends on the laser beam diameter and energy distribution, layer thickness, border overcure and, to a degree, recoater blade speed. Its illustration compares sidewalls built at 150 µm (0.006 in) layers. Vertical walls, upward faces and downward faces of one SLA master can therefore read differently, and each face carries its own roughness into the mold.
Machined masters come from model boards. Sika’s brochure offers medium-density polyurethane boards for master models, and singles out SikaBlock PROLAB 65 N, density 0.78 g/cm³ (48.7 lb/ft³), as having the smoothest surface aspect in its category, while its M600 N and M700 N boards are offered for the highest dimensional accuracy. No sheet on file prints a roughness value for a machined board surface, so a CNC master’s finish is measured on the master.
| Stage | What sets the surface | From the documents |
|---|---|---|
| Master process | build or machining process and orientation | SLA 4.075, MJF 14.548, FDM 22.075 µm Ra as built (Mustafa); SL sidewall set by beam, layer, overcure, recoater (Pang et al.) |
| Master finishing | sanding, sealing, priming, vapor smoothing | vapor-smoothed FDM gave a 0.340 µm cavity (Singh); masters sealed and smoothed, primer shown on an SLA master (Aggenbacht) |
| Parting tape | tape thickness on the master | tape of about 150 µm (0.006 in) leaves an error of its own thickness in the cast part (Aggenbacht) |
| Silicone | cure chemistry and surface | addition cure, virtually no shrinkage (Mustafa); high surface quality for clear parts (Sika SI291); condensation cure can haze clear castings (Polytek) |
| Mold frame | smoothness of the frame walls | a smooth frame gives a transparent mold, which helps cut a clean parting line (Aggenbacht) |
| Release agent | amount sprayed into the mold | too much release agent influences surface finish and strength (Aggenbacht) |
| Mold temperature and cure | oven settings | preheated molds improve surface quality (Polytek); cure temperature and time significant for Ra (Singh, Mustafa) |
What Casting Settings Change, and by How Much
Both studies ran designed experiments on casting settings and found effects, but small ones beside the master. In the Singh study, the polyurethane grade, the hardener percentage and the curing temperature were the significant terms for roughness, with the lowest roughness at a curing temperature of 70 °C (158 °F) and the full hardener ratio. Their Axson PX223 castings were smoother than those in Renishaw 6130 across the runs.
In the Mustafa study, the mold was preheated at 65 °C (149 °F) and three settings were varied: preheating time from 30 to 45 minutes, vacuum time from 15 to 21 minutes and curing time from 45 to 65 minutes. Curing time contributed 48.40 % of the variation in roughness. Yet all FDM castings stayed within Ra 21.445 to 22.025 µm (844 to 867 µin), and optimization reduced roughness by only 1.62 %.
The practical reading for a buyer is about proportion. A well-run casting process holds the surface to within a few percent of the master and keeps one batch consistent.
It does not polish a part. Polytek’s clear-resin bulletin points the same way from the maker’s side: preheated molds, at 66 °C (150 °F) in its example, reduce shrinkage and improve the surface quality of the casting, and vacuum degassing with pressure casting is what produces bubble-free parts. Loughborough’s guide lists bubbles among the things that can spoil the surface.
Casting settings move Ra by a few percent; the master moves it by a factor of five or more. A buyer who wants a finer cast surface asks for a finer master.
Measuring Ra on a Cast Part Under ISO 21920
The two studies measured with a stylus at 0.5 mm/s (0.02 in/s) and a cut-off of 0.25 mm (0.010 in). That setting matters when their numbers are set beside a drawing, because the current ISO rules tie the filter to the roughness being checked. Polytec, a maker of optical measuring instruments, explains the ISO 21920 series in a published guideline: ISO 21920-1 replaces ISO 1302 for drawing indications, ISO 21920-2 replaces ISO 4287 for the parameters, and ISO 21920-3 replaces ISO 4288 for measurement conditions.
Under ISO 21920-3, as the guideline reproduces it, the filter settings for Ra follow from the tolerance written on the drawing, through five setting classes.
| Setting class | Ra on the drawing | L-filter and section length | Evaluation length (5 sections) | Vacuum cast values that fall here |
|---|---|---|---|---|
| Sc1 | up to 0.02 µm (0.8 µin) | 0.08 mm (0.003 in) | 0.4 mm (0.016 in) | none |
| Sc2 | over 0.02 to 0.1 µm (0.8 to 3.9 µin) | 0.25 mm (0.010 in) | 1.25 mm (0.049 in) | none |
| Sc3 | over 0.1 to 2 µm (3.9 to 79 µin) | 0.8 mm (0.031 in) | 4 mm (0.157 in) | vapor-smoothed master and its castings, 0.3 to 1.7 µm |
| Sc4 | over 2 to 10 µm (79 to 394 µin) | 2.5 mm (0.098 in) | 12.5 mm (0.492 in) | SLA master and castings, about 3.6 to 4.1 µm |
| Sc5 | over 10 µm (394 µin) | 8 mm (0.315 in) | 40 mm (1.575 in) | MJF and FDM masters and castings, about 13.5 to 22 µm |
Every value in Table 1 was measured at the 0.25 mm (0.010 in) cut-off of class Sc2, while the classes their Ra values fall into call for 0.8 to 8 mm (0.031 to 0.315 in). A shorter filter leaves out longer waves of the surface, so a measurement made to the drawing’s class can read differently from the study’s figure on the same part. The studies remain sound comparisons of master against casting, because both were measured the same way; a drawing value is checked at the class the standard assigns.
The guideline adds two rules a buyer writes into an order knowingly. Unless otherwise specified, the maximum tolerance acceptance rule is now the default: one measured value beyond the limit rejects the sample. The 16 % rule, under which a share of readings may exceed the limit, has to be requested explicitly, and ISO 21920 introduces a new graphical symbol so that the two cannot be confused on a drawing.
Under ISO 21920-3, the Ra written on a drawing sets the filter used to check it. Cast surfaces from SLA masters fall in class Sc4 and from FDM masters in Sc5, so a drawing Ra for a cast part is measured with a 2.5 mm or 8 mm filter, not the 0.25 mm of the studies.
Gate, Vent and Parting Line Marks on a Cast Surface
A cast part also carries marks that its master did not have, and they belong in the finish specification. The Aggenbacht dissertation describes them in the order they are made.
- The gate. A rod glued to the master forms it, often joined through a small triangular piece so that the gate breaks off cleanly and needs little finishing. For parts up to 50 g (1.8 oz) of resin an 8 mm (0.31 in) gate is suggested.
- The risers. Brass rods of 2 to 3 mm (0.08 to 0.12 in) form them, or they are drilled through the mold afterward at 3 mm, and each leaves a small witness where it meets the part.
- The parting line. It is cut in two zones: a wave-like outer cut that keys the mold halves together, and a straight cut close to the part.
The parting line is where most of the visible work sits. According to the dissertation, the soft silicone it had available left clear parting lines on the cast parts, which affected the measured dimensions, and expected harder silicones to do better. Loughborough’s guide describes trimming the feed, the vents and any flash at the split line with pliers or a knife after demold.
For a buyer, that means the note on cosmetic faces also names where the parting line, gate and vents may sit. Loughborough’s advice is to bring the feed in at the lowest point of the mold, on a non-cosmetic surface and preferably into a thick wall.
Clear Parts and Polished Surfaces
Clear castings show every flaw of the master and the mold, which is why makers write about them separately. Sika lists easy polishing among the benefits of its clear grades PX522 and PX523, so a clear cast part can be brought up after demold as well as copied from a polished master. The PX523 sheet adds a limit that touches the finished look: to prevent yellowing, curing time is not to exceed 7 days at 70 °C (158 °F), 48 hours at 80 °C (176 °F) or 16 hours at 100 °C (212 °F).
Specifying Surface Finish for Vacuum Cast Parts
A drawing note that names a roughness for a cast part works best when it reflects how the finish is made, and when it is read under the measuring rules set out in the section above.
- Put the finish on the master first. Ask for the master’s Ra on the faces that matter, measured before the silicone is poured, since the part follows it.
- Name the faces. An SLA master’s vertical walls and top faces can differ; the note names the cosmetic faces and lets the others follow the build.
- Leave room for the parting line and gates. The Aggenbacht dissertation describes the parting line cut close to the part and the tape error at the split; Loughborough’s guide advises putting the feed on a non-cosmetic surface.
- For clear parts, ask about the silicone. An addition-cure mold and a polished master are the two conditions the makers name.
- Measure the first article. With a stylus, at the stated cut-off, on the faces named. In the 2020 study three castings agreed to within about 0.2 µm (8 µin) on the SLA master’s parts.
When the Cast Surface Is Changed After Demold
Some finishes are set deliberately in the mold rather than by the master. Smooth-On describes powder-coating a mold with a fine filler after the release agent: the casting comes out with a dry, matte finish and no release agent to remove, ready for primer. That is a texture chosen for painting, not for a bare part.
Other finishes come after demold: sanding, bead blasting, priming and paint. They change the surface completely and belong to the painting and texturing done after demold. For a bare cast part, the surface the buyer receives is the master’s, and the decision that controls it is made before the first gram of silicone is mixed.
Where a part’s surface is fixed by its master and needed in tens or hundreds of copies, the work fits low-volume vacuum casting, and a well-finished master can keep that surface consistent through bridge production while the steel tool, with its own polish or texture, is made.
Sources and Further Reading
- N. N. Mohd Mustafa, A. Z. Abdul Kadir, N. H. Akhmal Ngadiman, A. Ma’aram, K. Zakaria, Comparison of different additive manufacturing patterns on the performance of … vacuum casting for mating parts via the Taguchi method, Journal of Mechanical Engineering and Sciences 14(1), 2020, Universiti Malaysia Pahang
- J. Singh, R. Singh, H. Singh, Experimental investigations for dimensional accuracy and surface finish of polyurethane prototypes fabricated by indirect … tooling, a case study, Progress in Additive Manufacturing 2, 2017, Springer Nature
- Vacuum casting in the Loughborough Design School, a guide for final year students, R. Bibb, Loughborough University
- Development and evaluation of a vacuum casting process, F. C. Aggenbacht, M.Tech. dissertation, 2004, Central University of Technology, Free State
- T. Pang et al., SL 5410, high humidity, water and heat resistant resin for stereolithography, Solid Freeform Fabrication Symposium, 1997, University of Texas at Austin
- Brochure: Vacuum casting systems, H-5800-0110-03-A, issued 10.2017, Renishaw
- Move your business forward with SikaBiresin and SikaBlock solutions, tooling and composites, Sika
- Poly-Optic 14-Series casting resins, technical bulletin, Polytek Development Corp.
- What paint should I use and how can I make paint stick to my resin castings?, Smooth-On
- Roughness evaluation according to ISO 21920, how to read and comply with the latest standard, guideline, Polytec
- SikaBiresin PX522 with PX521, product data sheet, version 01.01, 08-2026, Sika