The Sika data sheet for SikaBiresin PX331 prints “Shore D hardness 86” and sets a capital A beside the number. A reader in a hurry takes the letter for the Shore A scale, and a buyer who does so ends up comparing a hard plastic with a soft rubber. The A is a footnote marker that points to the post-cure line at the bottom of the sheet, and the scale is D.
Shore hardness is the first number a casting buyer reads on any resin, and it is also the most compressed. A single figure folds together a test method, a durometer type, a temperature, a cure state and a reading time. This piece reads the standards behind the figure, tabulates what they cover, and lists what a casting supplier is entitled to sign when it quotes hardness.
Hardness Standards Behind a Cast Polyurethane Shore Value
Three documents appear most often around cast polyurethane. ISO 868 is the plastics method named on the resin sheets, ASTM D2240 is the American test method that reaches rubber and some plastics, and ISO 48-4 is the rubber method that covers softer grades. Each describes an indentation test, in which a spring-loaded steel indenter is pressed into the surface and the depth of penetration is turned into a number.
ISO 868, in its 2003 edition, specifies the determination of indentation hardness of plastics and ebonite with two durometer types. Type A is used for softer materials and type D for harder materials. The method permits a reading of the initial indentation, a reading after a specified period of time, or both. Its abstract calls it an empirical method intended primarily for control purposes, and that no simple relationship exists between the indentation hardness it gives and any fundamental property of the material.
Shore hardness is a control number. It tells a supplier whether this batch matches the last one, and it does not predict stiffness, wear or strength.
ASTM D2240 reaches wider. It covers twelve types of durometer, named A, B, C, D, DO, E, M, O, OO, OOO, OOO-S and R, and it describes the procedure for thermoplastic elastomers, vulcanized rubber, elastomeric materials, cellular and gel-like materials and some plastics. The standard states that it is not equivalent to other indentation hardness methods and instrument types, and its significance section adds that the geometry of the indenter and the applied force mean no simple relationship exists between readings from different durometer types. A buyer who needs to compare a reading across types therefore asks for it on the type that matters, not for a conversion.
The third document, ISO 48-4:2018, covers the hardness of vulcanized or thermoplastic rubber using durometers of the A, D, AO and AM scales. It is the one a casting buyer meets when the resin is a rubber-like grade or when a mold silicone is under discussion.
The Scales and Classes in One Table
The documents divide the field by scale letter and by material, and the table lines up what each one covers, using the abstracts and scopes of the documents themselves.
| Standard | Scales or types | Written for | Reading options |
|---|---|---|---|
| ISO 868:2003 | A (softer), D (harder) | plastics and ebonite | initial indentation, after a specified time, or both |
| ASTM D2240 (D2240-15, reapproved 2021) | A, B, C, D, DO, E, M, O, OO, OOO, OOO-S, R | thermoplastic elastomers, vulcanized rubber, elastomeric and cellular materials, gels, some plastics | per type, not equivalent to other hardness methods |
| ISO 48-4:2018 | A (normal), D (high), AO (low and cellular), AM (thin test pieces) | vulcanized or thermoplastic rubber | per scale |
Two details stand out. ISO 868 recommends ISO 48 for softer materials where a specification is being written, which places the soft end of cast polyurethane in rubber territory. And ISO 48-4 lists a scale for thin test pieces, which matters when the part has a wall that a standard sample thickness does not represent.
What a Letter Means When It Follows the Number
A hardness value carries two letters, and they do not mean the same thing. The scale letter follows the word Shore and is part of the name, as in Shore D. A footnote letter follows the number and marks a condition, as in the A after 86 on the PX331 sheet. Sika uses the same footnote scheme for flexural modulus, tensile strength and heat deflection on that sheet, and the footnote reads post-cure at 70 °C for 1 hour plus 80 °C for 16 hours.
The distinction costs nothing to check and protects the buyer from a misreading that can pass a design review. A quote that says Shore A 86 describes a hard rubber, and a quote that says Shore D 86 describes a rigid plastic with a flexural modulus of 3,700 MPa (537 ksi).
Casting Material Sheets and the Hardness They Print
The sheets state hardness with different scales, different temperatures and different cure conditions, and the table keeps them separate. Every figure is the maker’s own.
| Material | Printed value | Standard named | Condition on the sheet |
|---|---|---|---|
| SikaBiresin PX331 | Shore D 86 | ISO 868 | post-cure 1 h at 70 °C (158 °F) plus 16 h at 80 °C (176 °F) |
| SikaBiresin PX205 | Shore D 70 | ISO 868 | post-cure 16 h at 80 °C |
| SikaBiresin PX522 | Shore D 85 | ISO 868 | post-cure 4 h at 80 °C plus 16 h at 100 °C (212 °F) |
| SikaBiresin PX523 | Shore D 86 | ISO 868 | post-cure 16 h at 100 °C |
| Sika PX 223 HT | Shore D 80 | ISO 868:2003 | post-cure 1 h at 70 °C, 1 h at 100 °C, 12 h at 110 °C (230 °F) |
| Renishaw 6230 | Shore D 83 | ISO 868, at 23 °C | no post-cure |
| Renishaw 8263 | Shore D 83 at 23 °C, 80 at 60 °C, 80 at 80 °C | ISO 868 | no post-cure |
| Renishaw 8020-2 | Shore A 60 | ISO 868, at 23 °C | no post-cure |
| Renishaw Vacusil 2000 (mold silicone) | Shore A 37 | not named | cured 24 h at 23 °C |
| Wacker ELASTOSIL M 4601 (mold silicone) | about 28 Shore A | not named | product page, no condition |
Three patterns appear. The rigid grades cluster between D 70 and D 86, with PX205 as the low outlier because it is built to resemble polypropylene and HDPE. Soft grade 8020-2 is stated on the A scale, which matches ISO 868’s rule that type A serves the softer materials. And the mold silicones sit lower still, between about 28 and 37 on the A scale, a long way from any part they make.
The Same Grade at Three Temperatures
Renishaw is unusual in giving three readings for 8263: Shore D 83 at 23 °C (73 °F), and 80 at both 60 °C (140 °F) and 80 °C (176 °F). The drop is three points of Shore D between 23 °C and 60 °C, and the flat line between 60 °C and 80 °C means the figure stops falling in that range on this grade. A part in service at 70 °C therefore carries a hardness near the lower figure, not the room-temperature one that every other sheet prints.
Sika’s PX331, PX205, PX522 and PX523 sheets print one value with no temperature, while 6230 and 8020-2 state 23 °C. For a part in a warm enclosure or a hot hand, the one-figure sheet is silent, and a buyer who needs the number at temperature asks for it.
Cure State Behind a Hardness Value
All five Sika sheets above state their hardness after a post-cure, with schedules that run from 16 hours at 80 °C for PX205 up to 14 hours across three steps for PX 223 HT. A casting house that delivers a part straight from a 70 °C demold delivers a part that has not yet had the post-cure the printed value assumes. The Sika text on PX331 says that further post-curing of the demolded part can improve the final mechanical properties, which tells the buyer where the gap lies.
Renishaw’s resins invert the problem. The sheets for 6230, 8263 and 8020-2 all state no post-cure, so the printed hardness belongs to a part that left the oven at the end of its in-mold cure. That is a simpler promise, and it comes with a different gap: the sheets do not say how long after demolding the reading was taken, which ISO 868 allows to be either the initial indentation or a reading after a set time.
Two questions follow for every hardness value:
- At what temperature was the reading taken, and does the part see a different one?
- After which cure did the sample reach the printed value, and is that the cure the delivered part has?
A Rubber-Like Grade Read Under the Same Standards
Renishaw’s 8020-2 shows the soft end of the same casting process. The sheet gives Shore A 60 at 23 °C under ISO 868, tensile strength of 8 N/mm² (1.16 ksi), elongation at break of 200 percent, and a tear strength of 11 to 12 in the unit the sheet prints, N/mm². It is described as very low in viscosity and ideal for thin wall sections on gaskets, seals and valves, with a mix ratio of 100 to 90, a pot life of 300 seconds for 100 g at 25 °C, a cure of 90 minutes in the mold at 70 °C and a typical shrinkage of 0.2 percent. The same sheet notes a minimum shot weight of 150 g, a figure a thin gasket quickly outruns.
A rubber-like part makes the standards’ limits concrete. Type A on a durometer reads a soft solid by indentation depth, and ISO 868 itself points to ISO 48 for the softer materials when a specification is written. A gasket that has to seal is also judged by compression set and recovery, which neither standard measures, and the sheet prints neither. Another dissertation grade, a black rubber-like resin from a different supplier, is described as Shore hardness A65 with good tear resistance, so the A scale carries a wide band of resins that behave very differently from one another.
The mold silicones add a second soft band, with Vacusil 2000 at 37 A and ELASTOSIL M 4601 at about 28. A reader who sees a part at 60 A and a mold at 37 A can confirm that the mold is the softer of the two, which fits the job of releasing a part with undercuts.
Checking a Hardness on the First Article
A hardness callout is checked on the first parts, and the order of the checks decides how much the number can be trusted:
- Confirm the cure state of the sample against the sheet, since a part measured before its post-cure reads under the printed value.
- Read at the stated temperature, with the part conditioned in the room for long enough to match it.
- Take several readings away from edges and thin ribs, and report them as a set instead of a single figure.
- Record the scale, standard and reading time next to the numbers, so the same check can be repeated on the next batch.
Those four steps use no equipment beyond a durometer and a clock, and they are the reason a hardness callout works as a batch-to-batch control, which is the role ISO 868 gives it.
What a Casting Supplier Signs With a Hardness
A hardness quoted on a drawing is a short contract, and the standards show what it has to contain to mean something. The scale and the standard come first, for example Shore D to ISO 868. Next comes the temperature of the reading, since Renishaw’s 8263 shows how much a grade can change. Third is the cure state of the sample, and fourth the reading time under ISO 868, because the method allows the initial indentation, a timed one, or both.
| Item | Why it matters | Where it is defined |
|---|---|---|
| Scale and standard | A and D are different ranges of the same instrument family | ISO 868, ASTM D2240, ISO 48-4 |
| Test temperature | the same grade can read differently warm and cold | stated on the resin sheet, as for 8263 |
| Cure state of the sample | post-cure changes the printed values | resin sheet footnote |
| Reading time | initial or after a specified period | ISO 868 |
| Where on the part | thin walls and curved faces can differ from a test plaque | agreed with the supplier |
The last row is not set by any document opened for this piece, and a buyer who cares about it writes it into the drawing note or the quote. Such a note can be short: a location marked on the drawing, the number of readings and the instrument type. A supplier that agrees to it has agreed to measure what the buyer will measure on receipt, which removes the most common source of a hardness dispute between two labs reading the same part.
Limits Written Into the Hardness Standards
The documents are clear about what they do not do. ISO 868 states that the method is empirical and meant for control, and ASTM D2240 states that results from one durometer type do not map simply to another. Neither gives a table that converts a reading into modulus, wear resistance or scratch resistance.
Three limits follow from the standards’ own wording:
- Hardness does not convert into modulus, wear resistance or scratch resistance, and neither document offers a table that does.
- A reading on one durometer type does not map onto another, so a type change restarts the comparison.
- The soft end of cast polyurethane sits where ISO 868 points to a rubber method, so a rubber-like grade can be specified under more than one standard.
The hardness figure on a sheet therefore answers a narrow question: did a sample of this resin, cured this way, measure so many units on this instrument at this temperature. It does not tell a buyer how a snap hook will flex, how a seal will recover or how a surface will scratch. Those answers come from the tensile, flexural and elongation figures on the same sheets, read with their own test methods, and from a sample part.
A drawing note that names scale, standard, temperature and cure state turns a hardness figure into a check a supplier can sign.
A sound reading for a drawing is to call out the scale, the standard and the test temperature, and to treat the number as an acceptance check between batches, not as a design input. When a program moves from a handful of parts to a run, low-volume vacuum casting holds the hardness steady by casting each batch from the same grade and the same post-cure, and the same callout then carries into bridge production when a hard tool takes over.
Sources and Further Reading
- AFNOR, ISO 868:2003, Plastics and ebonite, determination of indentation hardness by means of a durometer (Shore hardness), abstract
- ASTM International, D2240, standard test method for rubber property, durometer hardness, scope
- Estonian Centre for Standardisation and Accreditation, ISO 48-4:2018, rubber, vulcanized or thermoplastic, determination of hardness, part 4, scope
- Sika, SikaBiresin PX331, product data sheet, version 01.01, 08-2026
- Sika, SikaBiresin PX205, product data sheet, version 01.01, 08-2026
- Sika, SikaBiresin PX522 with PX521, product data sheet, version 01.01, 08-2026
- Sika, SikaBiresin PX523, product data sheet, version 02.01, 11-2026
- Sika, PX 223 HT, technical data sheet, version 01, February 2021
- Renishaw, Data sheet: vacuum casting resin 6230, issued 09.2015
- Renishaw, Data sheet: vacuum casting resin 8263, issued 05.2015
- Renishaw, Data sheet: vacuum casting resin 8020-2, issued 04.2018
- Renishaw, Data sheet: Vacusil 2000 silicone rubber, issued 10.2017
- F. C. Aggenbacht, Development and evaluation of a vacuum casting process, M.Tech. dissertation, Central University of Technology, Free State, 2004
- Wacker Chemie, ELASTOSIL M 4601 US A/B, product page