PolyurethaneFirst ArticleShrinkage

Dimensional Accuracy of Vacuum Cast Parts From SLA, FDM and MJF Masters

A cast copy follows its master within a small fraction of a millimeter, and the printed master is the larger source of error against the drawing.

A 3D printed master pattern in grey resin beside the vacuum cast black polyurethane copy made from it.

A battery cover drawn at 49.84 mm on its long dimension came out of the same silicone-mold process at 49.30 mm, 50.01 mm and 49.95 mm, depending on which 3D-printed master the mold was made from. The spread of 0.71 mm (0.028 in) belongs to a published 2020 study from the Universiti Teknologi Malaysia, and it makes a point that no data sheet can: the master is the first dimension of every cast part, and the casting process adds its own error on top.

The study reports its measurements to the thousandth of a millimeter and grades them on the ISO tolerance scale, which makes it one of the few public sources that gives a casting buyer real deviation numbers. This piece reads those numbers, sets them in tables, converts them to inches, and lists what the study cannot tell a buyer about another part.

How Accurate Vacuum Cast Parts Are in a Published Study

The authors cast a battery cover for an enclosure, a thin-walled part 1.5 mm (0.059 in) thick with two measured dimensions: section A at 26.84 mm (1.057 in) and section B at 49.84 mm (1.962 in), both from the CAD model. They made three masters of it by three additive processes: fused deposition modeling (FDM) in ABS, stereolithography (SLA) in a detailed white resin, and multi-jet fusion (MJF) in polyamide. From each master they cast copies in an addition-cure silicone mold, using a polyurethane that simulates ABS.

The headline result is a pair of numbers for the best-controlled FDM series: after the authors optimized their process settings, the cast parts averaged +0.038 mm (+0.0015 in) on dimension A and −0.049 mm (−0.0019 in) on dimension B relative to their own master. That is the casting step alone, at a scatter well under a tenth of a millimeter on features of 27 and 50 mm. The master’s own deviation from the CAD model is a separate number, and it is larger.

Vacuum casting copies its master closely. The accuracy of the cast part is the accuracy of the master plus a casting error of about a tenth of a millimeter or less, on a thin part of this size.

The study is explicit about the chain. It states that the dimensional accuracy of the final parts is influenced by the dimensional accuracy of the additive-manufactured pattern, and that production cost and lead time differ by master process as well. The work here concerns dimensions of one part, one resin and one silicone, and it is read below as an example with known limits, not as a rule.

Three Masters Against the CAD Model

Differences between each master and the CAD dimensions dominate the final result, and the authors reported them in millimeters.

Table 1. Master dimensions and their deviation from the CAD model, in millimeters, with inches in brackets
Master process Dimension A Deviation from CAD Dimension B Deviation from CAD
FDM (ABS) 26.704 (1.051 in) −0.136 49.352 (1.943 in) −0.488
SLA (detailed resin) 26.897 (1.059 in) +0.057 49.977 (1.968 in) +0.137
MJF (polyamide) 27.065 (1.066 in) +0.226 50.148 (1.974 in) +0.308
CAD model 26.84 (1.057 in) not applicable 49.84 (1.962 in) not applicable

Closest to the CAD model on both dimensions is the SLA master, and furthest on dimension B is the FDM master, which falls short by almost half a millimeter. Signs differ too: FDM comes out smaller than the model, and SLA and MJF come out larger. A casting house that scales a master for resin shrinkage assumes the master is right, and this table shows how often a printed master is not.

The three masters come from three different families of additive manufacturing: FDM is material extrusion in ABS, SLA is vat photopolymerization in a detailed white resin, and MJF is powder bed fusion in polyamide. Each family builds the surface differently, with filament layers, cured resin layers or fused powder, and the roughness figures later in the study follow that difference. A master from a fourth process, or from a machined block, would sit somewhere else in the table.

How the Authors Measured

Dimensions came from a Mitutoyo PJ300 profile projector, an optical comparator, and the deviation of each cast part was the cast dimension minus the master dimension. Roughness came from a Mitutoyo stylus tester with a speed of 0.5 mm/s, a cut-off length of 0.25 mm and a sample size of 5. Molds measured about 10.3 × 7.5 × 5 cm and were preheated to 65 °C, and the resin was an ABS-simulating polyurethane, Alchemix VC 3392, used at roughly 1.3 times the weight of the master. Added together, preheating, vacuum and cure took about 2.22 hours per casting. The master’s error is the first entry in the part’s error budget, so a 3D printed master that is off by a tenth hands that tenth to every copy before the casting step adds its own.

What the Casting Step Added

Cast parts follow their masters, and the casting step adds a second, smaller deviation whose sign depends on the master. Table 2 averages the three copies the authors report for each master and computes each part’s distance from the CAD model.

Table 2. Cast parts from three masters, three copies each, with the writer’s means and distances from the CAD model in millimeters
Master Dimension Mean of cast parts Deviation from master (study) Deviation from CAD (writer)
FDM A 26.742 +0.038 −0.098
FDM B 49.303 −0.049 −0.537
SLA A 26.922 +0.025 +0.082
SLA B 50.013 +0.036 +0.173
MJF A 26.948 −0.117 +0.108
MJF B 49.951 −0.197 +0.111

Two patterns show up. The casting step’s own deviation is under 0.05 mm for FDM and SLA masters, and it reaches −0.117 and −0.197 mm for MJF, where the cast part is smaller than its master by about the resin’s shrinkage on a bigger master. And the distance from the CAD model is dominated by the master: the FDM-based part is 0.54 mm short on dimension B, while the SLA-based part is 0.17 mm over.

The authors make the practical consequence explicit. Battery covers cast from the SLA and MJF masters did not interlock well with the cavity of the enclosure, because dimension B came out larger than the cavity and left no clearance. The authors conclude that replacement parts are best made with the same additive technology that made the original, and that a design tolerance is needed when different technologies are used.

IT Grades Calculated From the Measurements

Measurements in the study are graded against ISO 286-1, whose scope defines the ISO code system for tolerances on linear sizes of cylinders and of two parallel opposite surfaces and gives a standard selection of tolerance classes. To grade them, the authors compute a standard tolerance factor from the geometric mean of the nominal size range, using i = 0.45 times the cube root of D plus 0.001 D, with i in micrometers and D in millimeters, and divide each deviation by it. Evaluating that formula gives about 1.31 µm for the 18 to 30 mm range of dimension A and 1.56 µm for the 30 to 50 mm range of dimension B.

Table 3. IT grades the authors report for their casting series
Series Dimension A (18 to 30 mm) Dimension B (30 to 50 mm) Remark in the study
Nine trial runs, FDM master IT5 to IT11 across the runs, both dimensions IT5 to IT11 across the runs, both dimensions inconsistent grades before optimization
Optimized FDM series IT8 IT8 consistent grade after optimization
SLA master series IT7 IT7 best of the three
MJF master series IT11 IT11 worst of the three

Several statements in that table deserve care. The trial runs show how much the casting settings matter, since the same master and mold gave grades between IT5 and IT11. In the authors’ analysis of variance, curing time contributed 87.17 percent of the variation in deviation A, while preheating time contributed 65.77 percent of the variation in deviation B and curing time 32.02 percent. And the grade for the three masters follows the deviation from the master, not from the CAD model, since the formula takes the difference between the cast part and the master.

What the Nine Trial Runs Show

Preheating time, vacuum time and curing time were varied over nine runs. Across the runs in the authors’ table, the average deviation on dimension A ranged from 0.008 mm to 0.120 mm, and on dimension B from 0.017 mm to 0.246 mm. The text of the paper cites 0.106 mm as the maximum for A, which does not match the 0.120 mm in its own table, and the writer reports the table.

After optimizing to 50 minutes of preheating, 18 minutes of vacuum and 65 minutes of cure, the three confirmation parts gave deviations of 0.037, 0.040 and 0.038 mm on A and 0.045, 0.055 and 0.047 mm on B. The authors compute a reduction of 64.15 percent and 80.08 percent against the pre-optimization maximum. A reader should notice that the process window here is a research setting, with a cure of 65 minutes that is only one point on a range other makers print differently.

Surface Roughness Follows the Master

A cast part follows its master’s surface closely, and the study gives numbers. The masters measured Ra of 22.075 µm for FDM, 4.075 µm for SLA and 14.548 µm for MJF, and the cast parts measured 21.63 to 21.72 µm, 3.58 to 3.79 µm and 13.50 to 13.94 µm. That is a decrease of 1.84, 9.62 and 6.09 percent according to the authors.

High roughness values mark the FDM series, and the paper’s own comparisons cite other studies in which chemically smoothed ABS masters gave cast parts at 0.319 to 0.667 µm and 0.455 to 0.593 µm. The message matches the one for dimensions: the master sets the surface, and the silicone and resin add little. A buyer who needs a smooth part asks for a master that is smoothed, and then confirms the cast part against a measured value.

Why Dimension A Grew and Dimension B Shrank

Direction matters in the data. The authors define a positive deviation as expansion and a negative one as shrinkage, and in their nine trial runs dimension B shrank in every run, while dimension A expanded in seven runs and shrank in two. They offer the direction in which the resin fills the silicone mold as a possible reason, citing earlier work, and the data cannot confirm it from a single part.

An older source from a different continent shows the same pattern. Its 2004 dissertation measured lengths and diameters on a machined specimen cast in polyurethane and found that, as the cure temperature went up, the lengths moved toward the required size while the diameters moved away from it. Between them, the two sources agree that a part does not shrink by one number, and that the dimension along the fill path behaves differently from the one across it.

For a buyer, the consequence is a rule of thumb about measurement, not about prediction. A single deviation on one dimension says little about the others, and the first article is measured on every critical dimension and in two directions at least.

The Study Set Beside Resin Data Sheets

Resin makers print shrinkage as a percentage or a number of millimeters per meter, and the study’s numbers can be put in the same units. On dimension B, the copies from the FDM master are 0.10 percent smaller than the master, those from the SLA master are 0.07 percent larger, and those from the MJF master are 0.39 percent smaller. Renishaw’s typical shrinkage figures for its ABS-like resins are 0.3 percent, and Sika prints 0.7 percent for two of its grades, so two of the three study results fall inside the printed range, and the SLA copies fall outside it on the growing side.

The positive sign for the SLA copies is the unusual one, since a resin that shrinks should give a smaller copy. In the trial runs, the authors attribute a growth in dimension A to the expansion of the mold at longer preheating time, and the heated silicone is a plausible cause for the SLA series too, although the paper does not say so. Nor does the text opened for this piece give the Alchemix resin’s own shrinkage figure, so a direct comparison with a maker’s value is not possible.

Preheating and Cure as Dimension Drivers

The statistics point at two process settings. Curing time dominated the variation of deviation A, and preheating time dominated the variation of deviation B. The authors’ reading is that deviation A rises with preheating time through the expansion of the mold, and that deviation B falls with preheating time and with curing time. Those are findings from nine runs and one mold, and they agree with the dissertation’s finding that mold temperature has an effect only above a threshold near 50 °C.

The practical use is modest. A casting room that wants stable dimensions fixes its preheating and cure times, records them, and does not change them between batches of the same part.

Drawing Notes for a Cast Mating Part

A mating part is the case where the numbers matter most. The study’s lesson fits in a short drawing note, and the note has four lines in practice, one for each of these points:

  • State which master process produced the master, and the measured size of the critical features on it.
  • Ask for the cast parts to be inspected on the same features, at one stated temperature, with the instrument named.
  • Give the fit as a tolerance grade on the feature, since ISO 286-1 gives the code system for linear sizes, and agree that grade for the cast part and not the master.
  • Keep the same master process for a later batch, since the study advises choosing the technology used for the original.

The cast part is only as good as its master. Measuring the master before the mold is made costs minutes and removes the largest source of error.

Limits of One Study for Another Part

The study is careful and also narrow. Four limits keep the numbers in their place:

  • It covers one part, a thin enclosure cover, and a size range from 27 to 50 mm. A larger or thicker part shrinks differently.
  • It uses one resin and one silicone, and the authors preheated the mold to 65 °C where resin makers print 70 °C.
  • It states the measuring instrument and the surface protocol but gives no measurement uncertainty for either.
  • Each cell has three copies, a small sample that cannot say how a mold behaves across 20 or 50 copies.

The honest use of the numbers is as an order of magnitude, which is also how the authors present them, as an early study that provides a base for later work. A cast copy lands within a tenth of a millimeter of its master on features of this size when the process is controlled, and the master can be off the CAD model by several tenths. For a mating part, the buyer asks for the master to be measured, not only the cast part, and for the first articles to be checked in the same way.

For parts where two printed or cast components have to fit, low-volume vacuum casting works from a measured master and a first article, and the measured values carry forward into bridge production as the reference for the next tool.

Sources and Further Reading

Send the Drawing of Your Cast Part

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Vacuum Casting chosen.

Request a Quote