OvenBatchPot Life

Making the Master Pattern for Vacuum Casting From SLA or CNC

The master is finished, sealed and fitted with its parting line, gate and risers before the silicone is poured, because the mold copies every mark into the batch.

Two master patterns of the same small housing, one CNC machined from white plastic and one SLA printed and sanded smooth in grey.

A strip of tape about 150 µm (0.006 in) thick, stuck along the master to mark where the silicone will be cut, leaves an error of exactly its own thickness in every part cast from that mold. The 2004 vacuum casting dissertation from the Central University of Technology, Free State, records it in one sentence, and the sentence sums up the whole operation. Everything on the master, including what is added to it for the mold maker’s convenience, is copied into the batch.

Making the master is the first step of the vacuum casting process step by step, and the one with the longest reach. This piece walks it in the order a model shop works: choosing the process, finishing and sealing, adding the parting line, gates and risers, and setting the master in its mold box. Each step has its figures and its typical failures, and each failure shows up in a specific place on the cast part.

What the Master Pattern Has to Deliver Before the Silicone Is Poured

A master pattern for vacuum casting is the physical original from which the silicone mold is cast, and the mold reproduces it so faithfully that every cast part inherits its shape, its surface and its faults. Loughborough University’s vacuum casting guide puts it plainly: the mold replicates the master extremely faithfully, so the master’s surface finish and accuracy are what the moldings will have. Renishaw’s vacuum casting brochure describes the cut mold as leaving a cavity that replicates the master perfectly.

The Free State dissertation by F. C. Aggenbacht lists what the master has to satisfy before anything else is done:

  • its mold has to fit inside the casting chamber;
  • the resin volume of the part has to fit the larger mixing beaker of the machine;
  • the master’s material has to be compatible with the mold silicone;
  • the part has to be simple enough for workable parting lines, because deep undercuts release badly and shorten mold life;
  • its thinnest walls have to suit the casting resin, since a resin too viscous for a thin wall will not fill it.

The first two are machine limits. In the dissertation’s own machine, a small facility handled 1,000 cm³ (61 in³) of plastic in a chamber of 450 × 450 × 350 mm (17.7 × 17.7 × 13.8 in); Renishaw lists mixing capacities up to 10 L (610 in³) for its systems. Loughborough adds a quick sizing rule for the mold itself: a bounding box around the part plus at least 5 cm (2.0 in) on each side.

A master is judged before it is finished: it has to fit the chamber, its resin has to fit the beaker, its material has to suit the silicone, and its walls and undercuts have to suit the resin and the mold.

Choosing Between an SLA Master and a CNC Master

Masters come from many processes. The Aggenbacht dissertation names handmade models and models grown by SLA, SLS or LOM, as well as CNC-machined models. Renishaw’s brochure calls stereolithography the most common source and notes that 3D printers of other kinds increasingly supply masters too.

Printed masters were compared directly in a 2020 study by Mustafa and co-authors at Universiti Teknologi Malaysia, who cast the same battery cover from FDM, SLA and MJF masters. The SLA master came out closest to the CAD model dimensionally and smoothest, at Ra 4.075 µm (160 µin) against 14.548 µm (573 µin) for MJF and 22.075 µm (869 µin) for FDM. A 2017 study by Singh, Singh and Singh reached a smooth surface from an FDM master instead, by exposing the printed ABS to acetone vapor for five cycles of 6 s each before the mold was made.

Machined masters are cut from model boards. Sika’s tooling brochure describes its medium-density polyurethane boards as the material for master models and molds for short series, with densities from 0.45 to 0.78 g/cm³ (28 to 49 lb/ft³). It singles out one board for surface and others for accuracy.

Table 1. Master pattern sources and what the opened documents report for each
Master source What the documents report Document
SLA lowest dimensional deviation of three printed masters; Ra 4.075 µm (160 µin) as built; most common master source Mustafa et al., 2020; Renishaw brochure
MJF (powder bed, polyamide) Ra 14.548 µm (573 µin) as built Mustafa et al., 2020
FDM (ABS) Ra 22.075 µm (869 µin) as built; smoothed in acetone vapor, five cycles of 6 s, to give a mold cavity of Ra 0.340 µm (13.4 µin) Mustafa et al., 2020; Singh et al., 2017
LOM to be sealed and skillfully worked by hand Aggenbacht, 2004
CNC from model board boards of 0.43 to 0.78 g/cm³ (27 to 49 lb/ft³); one board for smoothest surface, two for highest accuracy Sika brochure

The choice is less about the process name than about what the master carries into the mold. An SLA master arrives close to shape and smooth enough to finish in hours. A model board arrives as a block, takes a toolpath, and gives a dense, uniform surface with no layer lines; its limits are the board’s temperature range and the machinability of thin features. Neither study nor brochure on file compares an SLA and a CNC master on the same part, so the decision rests on the part’s geometry and surface. In practice the choice is between a 3D printed master that is sanded and sealed, and a master cut as machined plastic or model board, and each hands the silicone a different surface to copy.

Model Boards for CNC Masters

Sika’s brochure gives enough on its model boards to compare them as master materials, though some of its table columns are not printed for every board.

Table 2. Sika medium-density model boards for master models, as printed in the brochure (approximate values)
Board Density Temperature figure printed Brochure note
SikaBlock M450 N 0.43 g/cm³ (26.8 lb/ft³) service −30 to +70 °C (−22 to +158 °F) general-purpose board, lowest density of the five
SikaBlock ML45 PK 0.45 g/cm³ (28.1 lb/ft³) service −30 to +65 °C (−22 to +149 °F) superior surface quality, good edge stability
SikaBlock M600 N 0.60 g/cm³ (37.5 lb/ft³) heat deflection 77 °C (171 °F) easily workable, fine dense surface; highest dimensional accuracy with M700 N
SikaBlock PROLAB 65 N 0.78 g/cm³ (48.7 lb/ft³) heat deflection 90 °C (194 °F) smoothest surface aspect in its category
SikaBlock M700 N 0.70 g/cm³ (43.7 lb/ft³) heat deflection 78 °C (172 °F) good flexural strength and edge stability; highest dimensional accuracy

Most of these boards come in blocks of 1,500 × 500 mm (59 × 20 in), in thicknesses from 30 to 200 mm (1.2 to 7.9 in), and Sika lists adhesives (SikaBiresin B200, B260) and a filler (B370) for bonding blocks and repairing surfaces. A large master is therefore often a glued stack, and the glue line is a surface feature the mold will copy unless it is filled and finished.

The temperature line matters for the master’s life. A silicone mold cures around the master, and the dissertation notes that molds are cured and tempered at elevated temperatures; Renishaw’s brochure describes the mold being cured in an oven. Any board with a service limit of 65 °C (149 °F) sets the ceiling for any heat applied while it sits inside the mold.

Finishing and Sealing the Master

Finishing is where most of a master’s hours go, and the documents agree on its aim. The dissertation states that deficiencies in the master’s surface will be reproduced in the cast part, that the surface should be as smooth as possible and sealed, and that LOM masters in particular are to be sealed and worked off by hand. Its illustration shows an SLA master coated with primer before molding. Loughborough’s example shows an SLA master whose visible surfaces are highly finished and which is thoroughly cleaned before it goes into the mold box.

Clear parts raise the bar. The dissertation notes that the master’s finish influences the transparency of a clear casting, and Polytek’s bulletin for its clear casting resins asks for highly polished masters to create molds of excellent surface quality.

Printed masters bring two material questions with them. The first is resin stability. A 1997 paper from Ciba Specialty Chemicals and 3D Systems, on a stereolithography resin of that time, reported that earlier epoxy SL resins lost flexural modulus over days at 80 % relative humidity, while the newer resin kept it, and that its heat deflection reached 88 °C (190 °F) after a thermal post-cure at 80 °C (176 °F) for 2 hours. Each SL resin has its own figures, and a master that softens or creeps in a warm, humid shop changes shape before it is molded.

The second is hollow builds. Stratasys, in its guide to Somos SL patterns for investment casting, explains that SL patterns are often built hollow with an internal lattice and drain holes, that liquid resin is trapped inside and drained, and that the holes are placed where they can be plugged afterward. A hollow master for a silicone mold needs those holes sealed flush and its surface intact, or the plug becomes a mark on the part.

The master’s surface is finished, sealed and cleaned to the standard of the part. A printed master’s resin brings its own heat and humidity limits, and a hollow build brings drain holes to plug.

Parting Line, Gates and Risers on the Master

Before the silicone is poured, the master is fitted with everything the casting room will need, and each addition is copied too. The sequence in the dissertation and in Loughborough’s guide runs as follows.

  1. Mark the parting line. For uncomplicated parts the mold is cast in one piece and cut afterward. For complex parts, tape of about 150 µm (0.006 in) marks the line; Loughborough edges it in black so it shows through the silicone. The tape’s thickness becomes an error in the part, and it can also close through-holes so the mold halves separate.
  2. Or bed the master in clay. Deep undercuts call for a two-piece pour: half the master is embedded in a silicone-compatible clay, degassed, the first half of the mold is cast, the clay is removed and release agent is applied before the second half. Compatibility is checked by casting a little silicone onto the clay.
  3. Attach the gate. A rod glued to the master forms the gate. The dissertation suggests 8 mm (0.31 in) for up to 50 g (1.8 oz) of resin and 10 mm (0.39 in) for 50 to 100 g (1.8 to 3.5 oz), and a small triangular web where the rod meets the part so the gate breaks off cleanly. It goes to the lowest point of the cavity; Loughborough adds a non-cosmetic surface, preferably into a thick wall.
  4. Attach the risers. Brass rods of 2 to 3 mm (0.08 to 0.12 in) at the highest points let trapped air escape to the chamber. More can be drilled at 3 mm (0.12 in) through the finished mold.
  5. Tilt the master if it helps filling, so that the gate meets the lowest point and the risers leave from the highest.

Complex shapes take more than two pieces. Renishaw’s brochure notes that highly complex shapes are accommodated through multi-segment molds, and the dissertation describes cutting a mold into two or more sections to release the part, with the wave-like outer cut ensuring the pieces fit together only one way. Once the silicone has vulcanized, the master is freed by blowing compressed air through the gate and riser holes, which also eases its removal from the mold afterward.

Gates, risers, tape and clay are part of the master from the mold’s point of view. Their size, position and thickness are chosen on the master, because every casting repeats them.

The same steps are where a master’s later problems are made. A gate on a cosmetic face, a riser missing from a high pocket, or tape left on a datum face all show up on every casting, as a mark, an air trap or a step at the parting line.

Setting the Master in Its Mold Box

The last step before the silicone is building the frame around the master. Aggenbacht lists what the frame needs.

Table 3. Mold box and pour figures for a vacuum casting master, from the Free State dissertation and Loughborough’s guide
Item Figure Source
Silicone wall around the master at least 15 to 20 mm (0.6 to 0.8 in) for small parts, up to 100 mm (3.9 in) for large parts Aggenbacht
Mold size estimate bounding box of the part plus at least 5 cm (2.0 in) each direction Loughborough
Headroom for secondary degassing about 20 % extra height above the mold Aggenbacht
Degassing bowl for the silicone at least 5 times the silicone volume Aggenbacht
Silicone mixing ratio and pot life (4640 and 4642 silicones) 1:10 by weight; about 90 min at 23 °C (73 °F) and 50 % RH Aggenbacht
Vulcanizing before opening at least 15 h at room temperature Aggenbacht

The frame’s inner faces are smooth, so that the mold comes out transparent enough to see the parting tape when cutting; the dissertation found melamine board, joined with hot glue, quick to set up. It has to be stiff enough not to bulge while the silicone vulcanizes, and the master has to be supported firmly inside it. Loughborough’s guide warns that a leaking box wastes silicone and leaves irregularities in the mold.

Two cautions from the dissertation round off the step. If the frame sits in the vacuum chamber after the silicone’s pot life has expired, bubbles form under the top surface and stay there. A mold opened before every part of the silicone has hardened deforms where it is soft, and is lost.

What Goes Wrong With a Master and How It Shows on the Part

Because the mold copies everything, a master defect has a signature on the casting. The list below pairs the faults the documents name with where a buyer sees them.

  • Unsealed or porous surface (LOM, unsealed prints): texture and pores reproduced on every part.
  • Parting tape on the part’s surface: a step of about 150 µm (0.006 in) along the split.
  • Gate on a visible face: a trimmed witness on a cosmetic surface.
  • Missing riser at a high point: a short fill or air pocket in the same place on each casting.
  • Incompatible master or clay material: silicone that sticks or fails to cure against it, found when the mold is opened; the dissertation’s remedy is a small trial pour first.
  • Undercuts too deep for the mold: parts that tear or a mold that tears early, the dissertation’s warning on mold life.

The next steps start from here: measuring how closely the cast part’s surface finish follows the master, and scaling the master for the shrinkage of each resin. For parts needed in dozens to a few hundred copies from one well-made master, the work fits low-volume vacuum casting, and a second mold from the same master keeps a program running through bridge production while the hard tool is cut.

Sources and Further Reading

Send the Drawing of Your Cast Part

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Vacuum Casting chosen.

Request a Quote