Smooth-On’s support page on bonding urethane rubber to metal opens with a flat statement: urethane rubber will not stick to some metals, brass and stainless steel among them, under any circumstances. Brass is also the metal most threaded inserts are made from. PennEngineering calls C360 brass the industry standard for inserts, for its cost, conductivity and machinability.
Those two facts frame the whole job of putting an insert or a second material into a vacuum cast part. The insert is held by shape far more than by glue.
A bond between two cast layers depends on what is left on the first layer’s surface. And the resin has to be mixed and poured under vacuum around an obstacle that was not in the master. The steps below follow the order of the work, from designing the insert to demolding the second shot, with the figures each maker prints.
The Vacuum Casting Steps for a Part With Inserts
A vacuum cast part with molded-in inserts is made in eight steps: the insert is chosen and shaped for mechanical retention, the master is prepared so the mold can locate it, the insert’s surface is prepared, it is placed in the opened silicone mold, the mold is closed and preheated, the resin is degassed and mixed under vacuum, the mold is filled and vented, and the part is cured and demolded around the insert. An overmolded part adds a second mold and a second pour.
Loughborough University’s vacuum casting guide confirms that both are within the process. For fine details such as precise holes, it notes, metal mold inserts can be made, and with care and practice it is possible to overmold pins, bolts and nuts. The same guide warns that this is skilled work.
- Choose the insert for retention. Knurls, grooves and undercuts lock it into the cast resin.
- Prepare the master and the mold for location. The insert needs a seat in the silicone, a pin or a fixture that holds it where the drawing puts it.
- Clean and, where bonding is wanted, prime the insert. Oil and release agent prevent the resin from wetting it.
- Place the insert in the opened mold, seated on its pin, with no resin path into its thread.
- Close and preheat the mold to the temperature the resin’s sheet asks for.
- Degas the components and mix them under vacuum within the times the sheet prints.
- Pour, vent and let air back in before the pot life ends, so the resin is pushed around the insert.
- Cure, demold and check the insert’s position and the resin around it.
Inserts and overmolds in vacuum casting follow the casting cycle with three additions: a seat for the insert in the mold, a clean or primed insert surface, and a pour that fills around an obstacle the master did not have.
Designing the Insert for a Cast Thermoset
Cast polyurethane is a thermoset, and that rules out half the insert catalog. SPIROL’s design guide for threaded inserts states that thermoset plastics cannot be reformed by heat and pressure, so heat and ultrasonic inserts are not suitable for them; thermosets take molded-in, press-in or self-tapping inserts. PennEngineering says the same and ranks them: for a thermoset the best option is a molded-in insert, with press-in inserts a viable but lower-performance alternative.
Molded-in inserts hold by the resin flowing into their surface. PennEngineering describes them as designed to maximize outer surface area for pull-out and torque-out strength, with a diamond knurl along the length or a flat groove or undercut around the diameter to create a valley the plastic fills. SPIROL adds that helical knurls give the most torque resistance for a given diameter, that the volume of the knurls has to hold enough plastic to take the installation torque, and that the plastic trapped in the undercuts has to carry the pull-out load in service.
| Design point | Figure | Maker |
|---|---|---|
| Boss diameter or wall around the insert | about twice the insert diameter for best pull-out and torque-out | PennEngineering |
| Boss diameter or wall around the insert | two to three times the insert diameter, the multiple falling as the insert grows | SPIROL |
| Insert diameter against screw | generally twice the screw diameter, which raises the shear surface fourfold | SPIROL |
| Insert fit on its core pin | minor thread diameter held to a reduced tolerance for a good fit on the pin; countersinks ease placing | SPIROL |
| Resin kept out of the thread | blind-end inserts prevent plastic flowing inside | SPIROL |
| Core pin size | designed to compensate for plastic shrinkage | PennEngineering |
| Counterbore for a headed insert | 0.5 to 1.3 mm (0.02 to 0.05 in) larger than the head; depth at least the head thickness | SPIROL |
The insert makers write for injection molding, where a steel mold holds the insert on a core pin. In a silicone mold the pin is a metal pin seated in the rubber, or a fixture, and the principles carry over: the insert sits on a pin that matches its thread minor, a blind end or a tight fit keeps resin out of the thread, and enough resin surrounds it to resist the screw’s torque.
Preparing the Insert Surface
Mechanical retention does the heavy work, but the resin still has to wet the insert. The makers of urethane systems that bond to metal print what the surface needs.
| Step | Instruction | Maker |
|---|---|---|
| Choice of metal | urethane rubber does not stick to brass or stainless steel under any circumstances | Smooth-On |
| Mechanical key | etch or sand the metal | Smooth-On |
| Mechanical key, demanding repairs | blast to Sa 2½ near white, roughness 75 to 100 µm (0.003 to 0.004 in), angular disposable media, dry oil-free air | WEICON |
| Cleaning | free of oil, grease, dirt, oxides and residues; acetone, or the maker’s cleaner left to flash off completely, or the urethane will not cure fully | Smooth-On; WEICON |
| Primer | spray shellac as a bonding primer, or a dedicated adhesive primer | Smooth-On |
| Primer for aluminum | Sika Activator-205 to improve adhesion of its UR390 elastomer to aluminum | Sika |
| Timing | coat within one hour of preparation to avoid oxidation and new contamination | WEICON |
| Areas that are not to bond | treat with a silicone-free release agent | WEICON |
The brass statement matters for threaded inserts. A brass insert is held by its knurls and undercuts, not by adhesion, which is why the insert makers’ geometry in Table 1 is the real specification. Where a bond is wanted, on a steel or aluminum part for instance, the surface is keyed, cleaned and primed with a system made for that metal.
Cleanliness has a second reason in a urethane. WEICON’s sheet warns that a cleaner which has not fully flashed off leaves the urethane under-cured, and ResinLab’s technical bulletin explains why moisture is equally unwelcome: isocyanates react with water to form carbon dioxide, which leaves bubbles in the cured material. A wet or freshly wiped insert can therefore show a ring of bubbles in the resin around it.
An insert is held by knurls, grooves and undercuts. Where a bond is also wanted, the metal is keyed, cleaned until no solvent or moisture is left, and primed with a system named for that metal; brass and stainless steel are not bonded by urethane at all.
When a Post-Mold Insert Is the Better Choice
Molding the insert in is not the only way to get a metal thread in a cast part, and the insert makers set out the alternative fairly. SPIROL notes that installing inserts after molding shortens molding time, removes secondary cleaning, and reduces rejects and mold damage caused by dislodged inserts. In a soft silicone mold, where the insert sits on a pin in rubber rather than steel, that last point deserves weight.
For a thermoset, the post-mold options are press-in and self-tapping inserts. PennEngineering describes press-in inserts as favored for low-volume installations in less critical applications, at a cost in pull-out and torque-out, and recommends a larger boss to make up for it.
SPIROL adds that cold-pressed inserts need larger bosses or walls to withstand installation stress. Both makers ask for a hole deeper than the insert, two thread pitches beyond its length in PennEngineering’s guidance, and both prefer molded holes to drilled ones, since the dense surface of a molded hole holds better. In a vacuum cast part, a cored hole from a pin in the mold gives that molded surface.
A molded-in insert gives the best pull-out and torque-out; a press-in or self-tapping insert placed in a cored hole after demold costs performance but spares the silicone mold the risk of a dislodged insert.
Locating the Insert in the Silicone Mold
The insert’s position is decided by the mold, so the mold is made with the insert in mind. A 2004 vacuum casting dissertation from the Central University of Technology, Free State, describes the tools the mold maker already uses: rods glued to the master form gates and risers, and steel and brass rods form cavities in the silicone. That same technique gives a seat for an insert’s locating pin.
Two practical rules come from the same dissertation. Risers, 2 to 3 mm (0.08 to 0.12 in) brass rods at the highest points, let trapped air escape, and an insert creates new high points behind and under it where air can sit; extra risers can be drilled through the cured mold at 3 mm (0.12 in). Large molds may need support to keep them from distorting under their own weight, and a mold that sags moves the insert with it.
Where an insert is bought in, its own tolerances set what the mold can hold. SPIROL’s guide prints length tolerances of ±0.13 mm (±0.005 in) for its molded-in inserts, a reminder that the insert itself is a dimensional variable before the resin ever reaches it.
Mixing in Vacuum and Pouring Around an Insert
The pour is the same vacuum casting pour, with less room for error, because an insert narrows the flow path and creates corners for air. Resin sheets give the mixing sequence and its times.
| Item | Figure | Source |
|---|---|---|
| Degassing of components before mixing | wait 10 minutes at full vacuum (8040, 8045); 10 to 15 minutes (8060-2) | Renishaw sheets |
| Mixing time after cup A is tipped into cup B | 30 to 60 s (8040); 30 to 40 s (8060-2); about 45 s (PX 223 HT) | Renishaw; Sika |
| Mixing manner | as fast as possible without splashing | Renishaw sheets |
| Mold temperature | 70 °C (158 °F) preheat (Renishaw); 70 °C (158 °F) minimum (PX 223 HT) | Renishaw; Sika |
| Calming the mix | a pressure shot of 50 mbar (0.73 psi) let into the chamber if air still comes off | Aggenbacht |
| During the pour | a fast leak of about 25 % as the resin leaves the cup, then full release once resin rises in the vents | Loughborough guide |
| Resin quantity | part mass plus sprues plus at least 30 %, to keep a head of resin in the feed | Loughborough guide |
| Letting air in | before the end of the pot life, so air pressure pushes resin into the cavity | Renishaw sheets |
The dissertation describes the end of the pour from inside the chamber: when resin starts flowing out of the risers, the chamber is pressurized and the mold taken out to cure. Loughborough’s guide explains why the air is let back in: the vacuum removes air from resin and mold, and when it is released, air pressure forces the resin into the mold. Around an insert, that push is what fills the knurls and undercuts.
A thesis on bubble formation in cast polyurethanes, from Aalto University in 2025, adds why the vacuum level and timing matter. It cites a calculation in which existing bubbles expand to 50 times their size at 20 mbar (0.29 psi), and notes that pouring with a thin stream along the mold wall reduces trapped air. Bubbles left in the mix before the pour grow during the vacuum, so the degassing time in Table 3 is not shortened to save pot life.
Overmolding a Second Material Onto a Cast Part
Overmolding in vacuum casting is the same insert principle with a cast part as the insert. A first part, usually rigid, is cast and demolded; it is then placed in a second silicone mold whose cavity has the shape of the finished, overmolded part; and a second resin, often a rubber-like grade, is cast around it. Each mold comes from its own master, so the overmolded shape has a master of its own.
The documents on file give the conditions that decide whether the two shots behave as one part.
- Release agent off the first shot. Smooth-On writes that release agent on a casting makes painting almost impossible, and Polytek’s clear-resin bulletin tells users to wash mold release from surfaces before painting or bonding. The first shot is washed before it goes into the second mold.
- A clean first-shot surface. Smooth-On’s UreCoat is brushed onto cured urethane rubber after an alcohol wipe, as a permanent coating. Such a coating is not a cast second shot, and no opened document gives a bond strength between two cast urethanes, so the bond is judged on the first article; the cleaning rule carries over all the same.
- A second-shot grade chosen for the mold. Sika lists low aggressiveness on silicone molds among the reasons to choose its three-component PX840 rubber-like system, which covers the whole Shore A range; Renishaw’s 8891 covers 20 A to 90 A on its chart.
- The first shot fully cured. Polytek warns that parts demolded too soon may deform, and that thin sections cure more slowly than thick ones. A first shot that is still soft moves when the second resin is poured around it.
The second mold is made exactly like the first, with its gate and risers placed for the second resin. A two-piece mold technique in the Free State dissertation is useful here: it beds half the master in clay, casts one half of the mold, removes the clay, applies release agent to the first half and casts the second, so the parting line lands exactly where it is needed. In an overmold mold, that line is usually the boundary between the rigid and soft materials. The cast overmold usually previews a production part that will be injection molded in two shots or over an insert, so the order of steps and the bond tested here are the ones the mold maker will ask about.
Checking Inserts and Overmolds After Demold
A first article with inserts is checked for what the process can get wrong.
- Position. The insert’s location against its datum, since the silicone, the pin and the insert’s own tolerance all contribute.
- Thread cleanliness. Resin in the thread means the blind end or the pin fit failed.
- Voids around the insert. Bubbles in a ring around a wet or oily insert, or a short fill behind it where air was trapped.
- Retention. Pull-out and torque-out tested on sample parts, since both insert makers rest their figures on the resin trapped in the knurls.
- Bond line of an overmold. Peel at the edge of the soft material shows release agent or contamination left on the first shot.
Parts with inserts or two materials, needed in tens to a few hundred copies, suit low-volume vacuum casting, and the same molds and inserts can carry a program through bridge production until the insert-molded or two-shot production tool is ready.
Sources and Further Reading
- Vacuum casting in the Loughborough Design School, a guide for final year students, R. Bibb, Loughborough University
- Development and evaluation of a vacuum casting process, F. C. Aggenbacht, M.Tech. dissertation, 2004, Central University of Technology, Free State
- Threaded inserts for plastics, design guide, SPIROL
- Molded-in threaded inserts, PennEngineering
- What is a threaded insert?, PennEngineering
- I attempted to bond urethane rubber to stainless steel and it did not stick, FAQ 176, Smooth-On
- What paint should I use and how can I make paint stick to my resin castings? FAQ 141, Smooth-On
- UreCoat flexible urethane coating, technical bulletin, Smooth-On
- WEICON Urethane 60, technical data sheet, issued 18.02.2026, WEICON
- SikaBiresin UR390, product data sheet, version 02.01, 08-2026, Sika
- Move your business forward with SikaBiresin and SikaBlock solutions, tooling and composites, Sika
- PX 223 HT, technical data sheet, version 01, February 2021, Sika
- Data sheet: vacuum casting resin 8040, H-5800-0060-03-A, Renishaw
- Data sheet: vacuum casting resin 8060-2, H-5800-0597-03-A, Renishaw
- Renishaw vacuum casting resins and silicone rubbers, H-5800-0030-07-A, Renishaw
- Poly 15-Series liquid plastics, technical bulletin, Polytek Development Corp.
- Poly-Optic 14-Series casting resins, technical bulletin, Polytek Development Corp.
- Moisture contamination of polyurethanes, technical bulletin, ResinLab
- F. Parvinen, Mekaniska och kemiska processparametrarnas inverkan på bubbelformning vid formgjutning av polyuretaner, bachelor’s thesis, 2025, Aalto University