Sika prints the linear shrinkage of its PX205 casting resin as 7 mm per meter, and a reader who wants the figure for a 100 mm part divides by ten to get 0.7 mm (0.028 in). The same sheet specifies the bar that number was measured on: 3 mm thick, 50 mm wide and 250 mm long, cast in a silicone mold and post-cured for 16 hours at 80 °C. A buyer who forgets the bar applies a number from a slab to a rib or a boss, where the number may not hold.
Shrinkage is the tolerance driver that casting buyers meet first, and it is also one of the least standardized figures on a data sheet. This piece reads what the makers print, lines up the test bars behind each value, adds a measured series from a university dissertation, and turns percentages into millimeters on features of 25, 100 and 250 mm.
Linear Shrinkage Read as Millimeters Per Meter
Linear shrinkage is the fractional loss in length between the mold cavity and the cured part. A resin that fills a cavity 100 mm long and cures into a part that measures 99.3 mm has shrunk by 0.7 percent, which is the same as 7 mm per meter. The two units appear on different sheets, and one converts into the other by a factor of ten.
Two sources account for the loss in vacuum casting: the resin shrinks as it reacts and cools, and the silicone mold can change size as well. For the mold, the figures are small: the dissertation’s two silicones list a linear shrinkage under 0.1 percent after 7 days, and Wacker describes its ELASTOSIL M 4601 as non-shrinking. Almost all of the loss in a cast part therefore belongs to the resin, which is why the makers state the number per resin.
Shrinkage is a property of the resin on a particular bar under a particular cure. The same percentage applied to another shape is an estimate, and a first article is what confirms it.
The standards that organize measurement do not set the number. ISO 291 sets constant atmospheric conditions for conditioning and testing plastics, and ISO 1 defines a standard reference temperature for the specification of dimensional properties. A sheet that does not say at what temperature its bar was measured leaves a small uncertainty, since a 250 mm bar of a plastic changes in length with temperature, and the standards give the reader the convention to ask for.
Shrinkage Values Printed by the Makers
The sheets state shrinkage in three styles: as millimeters per meter on a named bar, as a percentage on a named bar, or as a typical percentage with no bar. Table 1 lines them up and converts each to a length lost on a 100 mm feature.
| Resin | Printed value | Bar or condition | Loss on 100 mm (3.94 in) |
|---|---|---|---|
| SikaBiresin PX205 | 7 mm/m | 3 × 50 × 250 mm bar (0.12 × 1.97 × 9.84 in), post-cure 80 °C for 16 h | 0.70 mm (0.028 in) |
| SikaBiresin PX522 | 7 mm/m | 500 × 50 × 5 mm bar (19.7 × 1.97 × 0.20 in), cure not stated on this line | 0.70 mm (0.028 in) |
| Sika PX 223 HT | 0 % after post-cure | 250 × 50 × 3 mm bar in a silicone mold, post-cure 70 °C for 1 h, 100 °C for 1 h, 110 °C for 12 h | 0.00 mm |
| Renishaw 6230 | typical 0.3 % | no bar named, no post-cure | 0.30 mm (0.012 in) |
| Renishaw 8263 | typical 0.3 % | no bar named, no post-cure | 0.30 mm (0.012 in) |
| Renishaw 8020-2 | typical 0.2 % | no bar named, no post-cure | 0.20 mm (0.008 in) |
| SikaBiresin PX331 | not stated | not applicable | not available |
| SikaBiresin PX523 | not stated | not applicable | not available |
Two features of the table are worth reading slowly. The two Sika values at 7 mm per meter come from bars with very different thicknesses, 3 mm and 5 mm, and the 0 percent of PX 223 HT comes from a 3 mm bar after a post-cure that reaches 110 °C. Renishaw gives its values as typical, and the sheets do not say whether they come from a bar, a part or a rule of thumb.
Why the Same Number Appears on Two Bars
PX205 and PX522 both print 7 mm per meter, and nothing on the sheets says the two resins shrink alike. The coincidence may reflect a rounded value or a common test procedure, since Sika’s sheets cite the same internal procedure number, CQP014-5, for both. A buyer using the figure on a thick part or a different shape carries the uncertainty that the bar’s thickness introduces, and asks for a measured value if the feature is critical.
Test Bars Behind a Shrinkage Number
A shrinkage bar is long and flat on purpose. Length makes the loss large enough to read with a ruler or a caliper, and the flat section keeps the cure uniform. A real part is rarely that shape, and the loss depends on the geometry in three ways that the bar hides.
Constraint is the first. A feature that surrounds a core in the silicone, such as the bore of a boss, cannot shrink freely, while an outside dimension can.
Cure heat comes second: a thick section reacts hotter and longer than a thin one, as the thickness-dependent demold times on the Sika sheets show. Direction is the third. A flowing liquid fills the cavity from the gate, and the dissertation reports differences between lengths and diameters, discussed below.
The standards are no help here. ISO 291 sets the conditioning atmosphere, and neither it nor any other standard opened for this piece defines a shrinkage test for cast thermosets. Each maker’s procedure is its own, which is why the table above lists bars and not a method name.
A Measured Series From a University Dissertation
A 2004 dissertation from the Central University of Technology in South Africa measured what a casting room gets in practice. The author used a machined steel specimen, made three silicone molds from it, cast polyurethane specimens in each, and took ten readings per dimension around each specimen with a micrometer that reads to 10 µm, averaging the three castings. Table 2 shows five of the eight dimensions he tracked, as the steel original and the average of the cast specimens.
| Dimension | Steel original | Cast average | Loss, mm | Loss, percent |
|---|---|---|---|---|
| Overall length L1 | 172.14 (6.777 in) | 170.69 (6.720 in) | 1.45 (0.057 in) | 0.84 |
| Long thin section L3 | 139.95 (5.510 in) | 139.54 (5.494 in) | 0.41 (0.016 in) | 0.29 |
| Diameter D1 | 28.98 (1.141 in) | 28.55 (1.124 in) | 0.43 (0.017 in) | 1.48 |
| Diameter D2 | 28.96 (1.140 in) | 28.78 (1.133 in) | 0.18 (0.007 in) | 0.62 |
| Diameter D3 | 9.68 (0.381 in) | 9.53 (0.375 in) | 0.15 (0.006 in) | 1.55 |
Several things show at once. The percentage differs by a factor of five between dimensions of the same part, from 0.29 percent on the long thin section to 1.55 percent on a small diameter. Lengths and diameters do not follow one rule. And the series carries its own scatter: the standard deviation across the thirty readings of the overall length, ten from each of three castings, was 0.36 mm.
The three casts also differ from each other. Averaging the ten readings on L1 gives 170.32 mm for the first cast, 171.10 mm for the second and 170.64 mm for the third, which are the writer’s sums from the printed readings. A spread of 0.78 mm on a 172 mm feature is about 0.45 percent, larger than the shrinkage figures that Renishaw prints for its resins, and the dissertation states that the deviation in the cast components was much bigger than in the original steel specimen.
What Moved the Number
The author varied three temperatures: the mold, the cure and the resin, which was held at 30 °C. Raising the cure temperature from 30 to 70 °C with the mold at 30 °C cut the shrinkage of the overall length from 0.8 percent to 0.4 percent. With the mold at 50 °C, the lengths again moved closer to the required size as the cure temperature rose, by about 0.5 percent, while the diameters moved further away by 0.2 to 0.3 percent. When the mold ran at 70 °C, the lengths showed a slight increase in shrinkage at a 50 °C cure and a decrease again at 70 °C, and the diameters showed a steady increase.
Mold temperature on its own gave a clear message only below a threshold. Between 30 and 50 °C the shrinkage stayed constant, and above 50 °C it began to vary, mostly toward less shrinkage on lengths. The dissertation’s own conclusion is that no clear pattern could be seen, since some dimensions rose while others fell when one condition changed, and that shrinkage in the order of 0.1 percent was obtainable by varying the casting conditions, with trial and error.
The dissertation’s lesson is practical: lengths and diameters respond to cure and mold temperature in opposite ways, so one scale factor cannot fix every feature.
From Percent to Millimeters on a Real Feature
A single multiplication turns the makers’ percentages into lengths. Table 3 does it for three feature sizes and four shrinkage values: the lowest printed (0.2 percent), the typical Renishaw value (0.3 percent), the Sika bar value (0.7 percent) and the dissertation’s overall length (0.84 percent).
| Shrinkage | 25 mm (0.98 in) | 100 mm (3.94 in) | 250 mm (9.84 in) |
|---|---|---|---|
| 0.2 % | 0.05 mm (0.002 in) | 0.20 mm (0.008 in) | 0.50 mm (0.020 in) |
| 0.3 % | 0.08 mm (0.003 in) | 0.30 mm (0.012 in) | 0.75 mm (0.030 in) |
| 0.7 % | 0.18 mm (0.007 in) | 0.70 mm (0.028 in) | 1.75 mm (0.069 in) |
| 0.84 % | 0.21 mm (0.008 in) | 0.84 mm (0.033 in) | 2.11 mm (0.083 in) |
At 25 mm the largest loss is a fifth of a millimeter, and at 250 mm it passes 2 mm. The table also shows why a flat percentage tolerance does not work: ±0.1 mm on a 250 mm feature is 0.04 percent, well under the scatter that the dissertation measured between casts.
Scaling the Master and Where It Stops Working
The usual response to shrinkage is to enlarge the master by the loss. A master for a part that shrinks by a fraction s is made 1 divided by (1 − s) times larger than the drawing. For 0.7 percent that gives 100.70 mm for a 100 mm feature, for 0.3 percent 100.30 mm and for 0.2 percent 100.20 mm.
A uniform scale fixes the average, and the average is only a number to aim at, since it is built from the loss at the cure the sheet describes and not from the cure of the day.
It does not fix a feature that shrinks 1.5 percent beside one that shrinks 0.3 percent, and the dissertation measured that spread inside one part. A scaled master also grows every wall and every gap by the same fraction, so a mating pair of features that matched on the drawing can drift apart. The cure and mold temperatures both moved the measured shrinkage in the dissertation’s series, so a production plan records the cure, mold and resin temperatures for every batch. For parts where two surfaces have to meet, the first article decides whether to correct one feature at a time on the master.
Cooling From the Oven to the Inspection Room
A cast part leaves the oven warm, and a second, smaller contraction waits in the cooling.
Two sheets print an expansion coefficient that lets the loss be estimated. Sika’s PX 223 HT lists 115 ppm per °C (64 ppm per °F) under ISO 11359-2, and Renishaw’s 6230 lists 8 × 10⁻⁵ under JIS K 6911 without a unit, which is read here as per °C. For a feature 100 mm long, cooling from the 70 °C of the mold to a 20 °C inspection room is a drop of 50 °C, and the part loses about 0.58 mm (0.023 in) on PX 223 HT and about 0.40 mm (0.016 in) on 6230. Both figures are the writer’s arithmetic from the sheet coefficients, and the sheets do not quote them.
Over that 50 °C drop the cooling loss reaches a few tenths of a percent, the same order as the 0.3 percent that Renishaw prints. A shrinkage figure is therefore only comparable between parts that were measured at the same temperature, which is why the reference temperature of ISO 1 and the conditioning atmospheres of ISO 291 matter on a quality plan. Measured hot at demold, a part reads larger than it does after a night in the inspection room.
Checking Shrinkage on the First Article
The check takes an afternoon and uses a caliper and a stable room:
- Measure the critical features on the master at the inspection temperature, and record the temperature.
- Cast the first article in the intended grade, post-cure it as the sheet says, and let it cool to the same temperature.
- Measure the same features on the part, and compute the loss in percent on each one, not as an average.
- Correct the master only on the features that drifted, and record the correction beside the grade and cure.
That record is the number that replaces the printed shrinkage for the next batch, and it belongs to the grade, the cure and the mold that produced it.
Whether a silicone mold itself moves is the smaller question, and the sources give a short answer. Wacker’s page calls ELASTOSIL M 4601 non-shrinking, the dissertation’s two silicones list under 0.1 percent after 7 days, and the 2020 study chose an addition-cure rubber because it exhibits virtually no shrinkage. Distortion of a large tool under its own weight is a separate matter, which the dissertation raises as a reason to support large molds, and it is not a property of the rubber.
Questions to Put to the Maker on a Shrinkage Figure
A buyer who works from the printed values keeps four questions at hand:
- Which bar produced the figure, and how thick was it compared with the thinnest and thickest section of the part?
- Was the bar post-cured, and with which schedule, compared with the cure the delivered part gets?
- At what temperature was the bar measured, and at what temperature will the part be inspected?
- Is the figure a measured value or a typical one, and who stands behind it?
Whether a resin keeps the shrinkage printed on its sheet across the first and the fiftieth copy from one mold is not stated by any maker, and it is the number a buyer most often wants. The practical answer is a measured check of one critical dimension at the start, middle and end of a run, recorded against the first article.
For features that matter, low-volume vacuum casting treats the printed shrinkage as a starting scale for the master and confirms it on the first parts, and the same record travels into bridge production when a hard tool replaces the silicone.
Sources and Further Reading
- Sika, SikaBiresin PX205, product data sheet, version 01.01, 08-2026
- Sika, SikaBiresin PX522 with PX521, product data sheet, version 01.01, 08-2026
- Sika, SikaBiresin PX523, product data sheet, version 02.01, 11-2026
- Sika, SikaBiresin PX331, product data sheet, version 01.01, 08-2026
- Sika, PX 223 HT, technical data sheet, version 01, February 2021
- Renishaw, Data sheet: vacuum casting resin 6230, issued 09.2015
- Renishaw, Data sheet: vacuum casting resin 8263, issued 05.2015
- Renishaw, Data sheet: vacuum casting resin 8020-2, issued 04.2018
- Wacker Chemie, ELASTOSIL M 4601 US A/B, product page
- N. N. Mohd Mustafa, A. Z. Abdul Kadir, N. H. Akhmal Ngadiman, A. Ma’aram, K. Zakaria, Comparison of different additive manufacturing patterns on the performance of … vacuum casting for mating parts via the Taguchi method, Journal of Mechanical Engineering and Sciences 14(1), 2020
- F. C. Aggenbacht, Development and evaluation of a vacuum casting process, M.Tech. dissertation, Central University of Technology, Free State, 2004
- Estonian Centre for Standardisation and Accreditation, EVS-EN ISO 291:2008, plastics, standard atmospheres for conditioning and testing, scope