Data SheetPost-CureFirst Article

Painting and Texturing Vacuum Cast Parts After Demold

A cast urethane part is painted only after its release agent is washed off and its surface keyed, with flexible coatings on parts that bend.

Three vacuum cast housings of the same design after finishing, one primed light grey, one painted glossy red and one with a fine textured matte black paint.

Smooth-On tested more than 30 aerosol primers on its cast urethane plastics and found that most did not work, or worked poorly at best. The low-quality ones beaded up on the casting. Two stood out. That small trial, published in the company’s own support pages, explains why the paint shop is the step of vacuum casting for plastic parts where a good batch most often goes wrong: the part is right, and the coating will not hold to it.

Painting after demold is a sequence, not a spray. The release agent has to come off, the surface has to be keyed and cleaned, an adhesion promoter and a primer have to suit a polyurethane, and a flexible part needs a coating that flexes. Texture, when it is wanted, is set either in the mold or in the coating. The order below follows the paint shop’s day, with the figures the makers of the resins and coatings print.

Painting Vacuum Cast Parts Step by Step

A vacuum cast part is painted by removing the release agent, keying and degreasing the surface, applying an adhesion promoter where the substrate calls for one, priming, and then applying the color and clear coats, with flexible additives in every layer when the part bends. The car refinish makers write the sequence most completely, because they paint new plastic parts every day.

Novol’s technical instruction for painting plastics sorts new parts into categories, and its third, “new plastic parts, not coated with factory primer”, is the case of a fresh casting. Its steps, with their figures, form the backbone of Table 1.

Table 1. Preparing and painting a new, unprimed plastic part, from Novol’s technical instruction (category III), with the conditions it prints
Step Operation Condition printed
1 Remove the release agent by washing hot soapy water, wax-free detergent
2 Degrease plastics degreaser (PLAST 815)
3 Bake 60 °C (140 °F) for at least 30 minutes
4 Degrease again same degreaser
5 Scuff while degreasing gray 800 ultra fine scuff pad wetted with degreaser; blow off with compressed air
6 Degrease a last time same degreaser
7 Adhesion promoter one step (promoter added to an acrylic or epoxy primer) or two steps (promoter as its own layer, then primer)
8 Flexible parts elasticity agent (PLAST 775) added to every layer except the basecoat
9 Paint system per the data sheets of the chosen primer, base and clear

Three points of the table are worth reading closely for cast urethane. The bake at 60 °C (140 °F) between degreasing passes comes before any paint; its purpose is not stated, but it brings anything left in the surface out before the next wipe. Its scuff is fine, 800 grade, so the master’s surface is keyed rather than cut away. And the guide’s own rule of thumb is to use the adhesion promoter every time, because correcting paint costs far more than the promoter.

Painting a cast part follows the new-plastic sequence of the refinish trade: wash off release, degrease, warm, scuff fine, degrease, promote adhesion, prime, then color, with flexibility added to every layer of a soft part.

Removing Release Agent From a Fresh Casting

Release agent is the main enemy of paint on a casting, and both resin makers and coatings writers say so. Smooth-On’s FAQ states that using a release agent to free the casting from the mold makes painting it almost impossible, and that removing the agent is difficult and another labor step. An answer in Products Finishing, from consultant Carl Izzo, agrees that the release has to come off to ensure adhesion, and suggests asking the release agent’s maker which solvent removes it.

Polytek’s bulletins give the plainest instruction. Its Kast-Series bulletin says that when all mold release is removed by detergent washing, most oil paints work well, and its clear-resin bulletin repeats: wash mold release from surfaces before painting or bonding. Novol’s hot soapy water with a wax-free detergent is the same idea in a car shop’s words.

The silicone itself can add to the load. Sika describes one catalyst for its SI291 vacuum casting silicone as self-bleeding, giving an oily surface for better release and longer mold life. A mold that releases by oiling its own surface leaves that oil on the part, which is one more reason the wash comes first. The 2004 vacuum casting dissertation from the Central University of Technology, Free State, adds that release agent is sprayed into the silicone as a thin cloud, and that too much of it affects both the surface finish and the strength of the cast part.

Release cannot simply be dropped. Smooth-On notes that casting urethane resin in a silicone mold without release agent cuts the mold’s production life by half. The paint shop therefore inherits the release and plans to remove it.

Priming in the Mold Instead of After Demold

Two makers describe a way around the cleaning step: putting the primer into the mold so that it comes out bonded to the part.

Smooth-On’s method is to apply the release agent to the mold, then spray an auto body primer into the cavity, then cast the resin. The primer bonds to the casting’s surface and the part comes out ready for painting. Polytek says the same in its Kast-Series and 15-Series bulletins: an appropriate primer sprayed into a silicone mold and allowed to dry before casting gives a pre-primed part, and helps later paint adhere.

The method has limits a buyer should weigh. A primer layer copies the mold, so its thickness and evenness show on the part, and any run or dry spray in the cavity becomes a defect on every casting. It suits parts that will be painted anyway, and for which a uniform primer skin is acceptable.

When the primer goes on after demold instead, Polytek advises an auto body primer sprayed onto the clean casting and left to cure for at least 24 hours before paint. Smooth-On’s choice of acrylic paints for its castings, and its warning that some testing for paint compatibility may be necessary, close the sequence.

Painting a Part That Came Out of the Mold Primed

A casting primed in the mold is no longer bare plastic, and Novol’s instruction has categories for that case too. Its first two categories cover new parts that already carry a primer, one resistant to solvents and one sensitive to them. Two quick tests sort them before anything is sprayed.

  • Solvent resistance test. A small hidden area is wiped with the plastics degreaser. If the surface softens or turns sticky, the primer or plastic is not solvent resistant.
  • Sanding test. A light pass with P500 paper; fine dust on the paper points to a primer layer on top.
  • Solvent-resistant primer (category I). Degrease with the plastics or universal degreaser, scuff with fine paper or the gray 800 pad, blow off, degrease again, then paint.
  • Solvent-sensitive primer (category II). The solvent degreasers are left out, since they would strip the primer. A waterborne degreaser is used before and after scuffing.

The same instruction applies its flexibility rule in both categories: for a part made of flexible plastic, each layer of the paint system except the basecoat is made more flexible with the elasticity agent. A primer cast onto a rubber-like part is therefore still followed by a flexible system.

A part primed in the mold is tested before it is painted: a degreaser wipe and a light sanding show whether its primer tolerates solvents, and that decides which cleaner the painter uses.

The Clock Between Demold and a Painted Part

Painting adds hours that a buyer can plan from the figures on file. Novol’s bake is at least 30 minutes at 60 °C (140 °F).

Polytek asks for at least 24 hours of cure on an auto body primer sprayed after demold. A brushed urethane base like UreCoat takes 30 minutes between coats, 2 hours to become tack-free and 16 hours at 23 °C (73 °F) to cure fully, or 4 hours at 60 °C (140 °F). The cast part itself, per the Products Finishing answer, is generally fully cured as it leaves the mold, so the painting clock starts at demold once any post-cure in the resin’s sheet is done.

Adhesion Promoters and Primers for Cast Polyurethane

Not every plastic needs an adhesion promoter, and the refinish guides say which do. Novol notes that polypropylene and its blends cause the most problems in painting and are solved with promoters, while ABS, polycarbonate and PC/PBT are considered paintable without them. It then advises using the promoter anyway, as cheap insurance. PPG’s standard procedure for bare plastic makes it part of the routine: the part is cleaned and coated with adhesion promoter before the undercoat.

For cast urethane specifically, Smooth-On sells an adhesion promoter for its Maker Pro Paints that it describes as bonding to rigid urethanes, rigid urethane foams, epoxies and other rigid substrates. Its product page gives a coverage of about 56 m² (600 ft²) per US gallon at 30 to 38 µm (1.2 to 1.5 mil) dry film, in one thin coat, and adds a clear limit: the promoter is not used when painting flexible surfaces.

Table 2. Coating approaches for rigid and flexible cast urethane parts, as the opened documents give them
Part Approach Document
Rigid cast urethane adhesion promoter, then primer and acrylic paint Smooth-On Maker Pro adhesion promoter; Smooth-On FAQ 141
Rigid cast urethane, painted anyway primer sprayed into the mold before casting, part comes out primed Smooth-On FAQ 141; Polytek Kast-Series and 15-Series
Rigid cast urethane, primed after demold auto body primer on the washed part, cured at least 24 hours Polytek Kast-Series
Flexible part, general flexible coatings such as vinyl or polyurethane enamels Products Finishing, Izzo
Flexible plastic, refinish system elasticity agent in each layer except the basecoat Novol
Flexible plastic, refinish system flexible additive in undercoat and clearcoat, activator in the basecoat PPG PD-0200C
Urethane rubber or flexible foam flexible urethane paint base, colored, brushed in layers Smooth-On UreCoat

Primer choice is where Smooth-On’s trial of more than 30 aerosol primers matters. It names Dupli-Color Sandable Primer and Bulldog Adhesion Promoter as the two that gave excellent adhesion, whether applied to the mold surface or to cured castings without release agent. PPG adds what to do with surface flaws: a primer surfacer over scratches, or a flexible glaze filler, sanded, for deeper imperfections.

Painting Rubber-Like and Flexible Cast Parts

A rubber-like casting flexes, and a rigid coating on it cracks. The Products Finishing answer is direct: if the molded part will flex in use, flexible coatings such as vinyl or polyurethane enamels are prescribed; otherwise most commercial paints will adhere. It also notes that molded polyurethane is generally fully cured when it comes out of the mold and needs no further cure before painting, while all coatings themselves have to be cured.

Smooth-On’s UreCoat shows what a coating made for rubber looks like on paper. It is a two-component urethane brushed onto cured urethane rubbers or flexible foams as a permanent, colored paint base that bends with the part.

Table 3. Smooth-On UreCoat flexible urethane coating, handling and cured properties as printed
Property Value
Mix ratio 100 A : 10 B by weight
Pot life 8 minutes at 23 °C (73 °F)
Recoat time 30 minutes
Tack-free time 2 hours
Full cure 16 hours at 23 °C (73 °F), or 4 hours at 60 °C (140 °F)
Hardness Shore 70 A
Elongation at break 876 %
Humidity for application below 50 % relative humidity, to minimize bubbles
Coverage of a 4.08 kg (9 lb) unit 4.91 m² (52.8 ft²) at 0.8 mm (1/32 in)

Its preparation notes match the paint shop’s: porous or non-porous surfaces sanded and wiped clean with alcohol; urethane rubber wiped with alcohol and dried; metals sanded, cleaned and given two coats of spray shellac. The bulletin also warns that, like all urethanes, the coating is moisture sensitive, which is why it gives the humidity limit.

Flexible cast parts take flexible coatings: a promoter for rigid substrates is left off, flexible additives go into the primer and clear, or a urethane paint base made for rubber is used.

Texturing Vacuum Cast Parts After Demold

Texture on a vacuum cast part comes from one of three places, and only two of them are after demold. The first is the master: the silicone copies its surface, which is why a molded-in texture is set when the master is finished.

The second is the mold surface treatment. Smooth-On describes powder coating the mold: release agent is applied, then a fine filler powder, the excess is blown out, and the resin is cast. The casting comes out with a dry, matte finish and no release agent to remove, so it can be primed and painted at once. This method trades the master’s gloss for a uniform matte surface that takes paint well.

The third is the coating. UreCoat cures to a high gloss; for a matte look, Smooth-On offers a matting powder combined with solvent and the coating, which gives a lasting matte surface. Refinish primers and clears bring their own gloss levels, and the scuffing in Table 1 is fine enough, at 800 grade, to key the surface without leaving a visible texture.

The documents on file give no figures for bead blasting or sanding cast polyurethane to a set texture, so any such finish is agreed on a sample panel or a first article before the batch is painted.

What Goes Wrong in the Paint Shop and How It Shows

The makers’ warnings pair neatly with the defects a buyer sees on delivered parts.

  • Paint beading or lifting: release agent left on the part, or a primer not suited to urethane; Smooth-On’s primer trial and its FAQ describe exactly this beading.
  • Cracks in the coating of a soft part: a rigid paint system on a flexing part, or an adhesion promoter meant for rigid substrates.
  • Yellowing and chalking outdoors: Polytek states that its Kast-Series and LiteCast plastics yellow and chalk in sunlight and are to be painted or sealed for exterior use, with the coating’s adhesion checked over time.
  • Bubbles in a brushed urethane coating: humidity above the coating’s limit, 50 % relative humidity for UreCoat.
  • Static and dust in the finish: Novol recommends an antistatic degreaser and earthing all parts in the spray booth, which also lowers the risk of ignition from static discharge.

Some colors are better painted than cast in. Loughborough University’s vacuum casting guide lists, among the disadvantages of the process, that adding colorant to certain resins makes opacity difficult to achieve. A painted finish solves that, at the price of this whole sequence; a color matched in the resin before casting avoids it.

Painted vacuum cast parts in tens to a few hundred copies fit low-volume vacuum casting, where the paint shop works part by part, and the same coating system can carry a program through bridge production until molded parts take over.

Sources and Further Reading

Send the Drawing of Your Cast Part

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Vacuum Casting chosen.

Request a Quote