A 100 g batch of one ABS-like casting resin stays pourable for 6 minutes at 25 °C and for 3 minutes 40 seconds at 35 °C. Both figures sit on the same Renishaw data sheet for resin 6230, and the gap between them says more about how this family of materials behaves than any single strength value does. The resin is a two-component polyurethane that starts reacting the moment the components meet, so its working time, its demold time and its final properties all depend on temperatures the buyer rarely sees.
A buyer who asks for an ABS-like part is really asking for a thermoset that, on its datasheet, comes within reach of a thermoplastic. The sections below read four such grades from three makers side by side, show what the label does and does not promise, and list the conditions that sit behind each number.
Why a Polyurethane Resin Is Called ABS-Like
The phrase is a maker’s shorthand, not a standard. Sika describes its SikaBiresin PX331 as having mechanical properties similar to thermoplastics like filled ABS, and Renishaw lists its 6230 as having properties similar to ABS. Neither sheet names a reference ABS grade or a test report that ties the two together. The label therefore points at a region of the property map (hard, stiff, with limited stretch) rather than at a numeric match.
What the label does carry is a family resemblance in hardness and stiffness. Every grade read here lands between 80 and 86 on the Shore D scale, flexural modulus between 1,800 and 3,700 MPa (261 to 537 ksi), and elongation at break between 4 and 15 percent. Parts made from them are rigid and hard, which is the behavior a buyer expects from a molded engineering plastic.
An ABS-like resin is a thermoset chosen for its stiffness, hardness and heat deflection. The label names a use, and the numbers below carry the details.
Four grades make a fair sample: SikaBiresin PX331, Sika PX 223 HT, Renishaw 6230 and Renishaw 8263. They cover a general technical grade, a high-temperature grade, a milky-white grade with no post-cure and a flame-retardant grade for housings. The name points to the part’s future: an ABS-like casting stands in for a housing that will later be injection molded in real ABS, so the cast copies are judged against the thermoplastic the program is heading for.
Four ABS-Like Grades Side by Side
The table gives each maker’s printed value in the maker’s unit, with the converted value beside it. Blank cells mean the sheet does not state the property, and a note after the table lists the conditions each figure depends on.
| Property | PX331 (Sika) | PX 223 HT (Sika) | 6230 (Renishaw) | 8263 (Renishaw) |
|---|---|---|---|---|
| Shore D hardness, ISO 868 | 86 | 80 | 83 (at 23 °C) | 83 (at 23 °C), 80 (at 60 and 80 °C) |
| Flexural modulus | 3,700 MPa (537 ksi) | 2,300 MPa (334 ksi) | 1,800 MPa (261 ksi) | 2,200 N/mm² (319 ksi) |
| Flexural strength | 133 MPa (19.3 ksi) | 80 MPa (11.6 ksi) | 80 MPa (11.6 ksi) | 93 N/mm² (13.5 ksi) |
| Tensile strength | 55 MPa (8.0 ksi) | 60 MPa (8.7 ksi) | 67 MPa (9.7 ksi) | 68 N/mm² (9.9 ksi) |
| Elongation at break | 4 % | 11 % | 14 % | 15 % |
| Heat deflection temperature | 90 °C (194 °F), ISO 75A | not stated | 98 °C (208 °F), ISO 75 at 1.80 MPa | 80 °C (176 °F) |
| Glass transition | 100 °C (212 °F), ISO 11359 | 120 °C (248 °F), TMA | 115 °C (239 °F), TMA | not measured |
| Shrinkage as stated | not stated | 0 % after post-cure, 250 × 50 × 3 mm bar | 0.3 % typical | 0.3 % typical |
Reading across, PX331 is the stiffest and strongest in bending, while the Renishaw grades stretch further before they break. The stiff end is also the brittle one: PX331 reaches 4 percent elongation at break and 26 kJ/m² impact resistance on Sika’s ISO 179 test, and 6230 gives 15 kJ/m² Izod. Those two impact figures come from different methods and notch types, so the sheets cannot rank the grades on toughness.
Which Figure Comes From Which Cure
Only some of the values describe the part a buyer receives. Sika’s PX331 values are stated after a post-cure of 1 hour at 70 °C followed by 16 hours at 80 °C. The PX 223 HT figures assume 1 hour at 70 °C, 1 hour at 100 °C and 12 hours at 110 °C. Renishaw’s 6230 and 8263 list no post-cure at all, which means their figures describe a part straight out of the 70 °C oven.
A part delivered without the post-cure Sika lists for PX331 is therefore not the part its datasheet describes. The same grade can read as Shore D 86 on the sheet and measure lower on a part demolded at 45 minutes and shipped.
Oven Temperatures, Pot Life and Demold Time by Grade
Every grade in the table is cast at room-temperature conditions into a silicone mold at 70 °C, and every sheet leans on temperature in a different place. Sika asks for material and processing temperature between 18 °C and 25 °C. Renishaw heats the resin to 35 to 40 °C for 6230 and 40 °C for 8263, after storing the unopened cans in an oven at 70 °C for 2 hours and then at 40 °C.
| Figure | PX331 | PX 223 HT | 6230 | 8263 |
|---|---|---|---|---|
| Mix ratio by weight, A to B | 100 : 100 | 100 : 80 | 100 : 200 | 100 : 150 |
| Pot life | 6 min (200 g, 23 °C) | 6 to 7 min (90 g, 25 °C) | 6 min (100 g, 25 °C); 3 min 40 s (100 g, 35 °C) | 360 s (100 g, 25 °C) |
| Mold temperature | 70 °C (158 °F) | 70 °C minimum | 70 °C | 70 °C |
| Demold time | 45 min above 3 mm; 75 min below 3 mm | 45 to 70 min | 25 to 60 min | 60 min in mold |
| Maximum casting thickness | 5 mm (0.20 in) | 5 to 10 mm (0.2 to 0.4 in) | not stated | not stated |
| Post-cure | 1 h at 70 °C plus 16 h at 80 °C | 1 h at 70 °C, 1 h at 100 °C, 12 h at 110 °C | none | none |
Two details in the table deserve a second look. The pot life depends on the batch size, because a larger mass keeps more of its own reaction heat, so the Sika sheet for PX331 states it for 200 g while the PX 223 HT sheet states it for 90 g. And the thin-wall case runs longer on PX331, at 75 minutes below 3 mm, which is the opposite of what a buyer expects until the chemistry is in view: a thin wall holds less of its own reaction heat and leans on the oven, which is a reading of the sheet, not a statement in it.
Reading a Pot Life Before Ordering a Large Part
The pot life limits how much resin one pour can carry. When the cavity needs a volume that cannot be poured in 6 minutes, the mold is filled in sequence or a slower grade is chosen. The sheets give mass, not volume, and an ABS-like resin at 1.2 to 1.35 g/cm³ (75 to 84 lb/ft³) turns 200 g into roughly 150 to 165 cm³ (9 to 10 in³). That is the amount a single mix of PX331 can hold before the clock runs out.
Thickness Windows and Why Thin Walls Cure Differently
Each grade carries a thickness ceiling because the reaction releases heat. Sika limits PX331 to 5 mm (0.20 in) and gives PX 223 HT a window of 5 to 10 mm (0.2 to 0.4 in). The sheets do not explain the cap, but the reaction heat of a thick section is the likely reason, and the cap is the thickest section the maker tested.
The thin side matters as much. A wall under 3 mm needs longer in the oven on PX331, and the Sika sheets advise supporting heavy or thin parts on a conformer, a fixture shaped like the part, while they post-cure. The PX 223 HT sheet is blunter: after demolding the part is to be supported in the oven so it keeps its shape, and the geometry and mass of the part are to be checked for deformation risk. A part that looks straight at demold can bow during a 16-hour soak at 80 °C if nothing holds it.
Thickness decides three things on an ABS-like resin: whether the grade can fill the section at all, how long the part stays in the oven, and whether it needs a conformer for post-cure.
Flame Retardancy and Coloring in the Same Grades
Two grades carry a flame rating. Sika states a UL 94 rating of V-0 at 3 mm for PX331, a V-0 result at 3 mm under NF EN 60695-11-10, and compliance with the FAR 25 §853 (b) aviation standard at 1.5 mm. Renishaw describes 8263 as certified fire retardant to UL 94 V-0 and suggests electrical enclosures as its use. The standards behind those lines are treated in these resources’ standard piece on UL 94 for cast polyurethane.
Coloring has limits too. Sika recommends adding 1 percent pigment to the polyol, using its own color pastes that are tested with these systems, and keeping the pigment free of moisture. Renishaw states a ceiling of 2 percent colorant by total weight for 6230 and 8263, added to the A component before mixing. Moisture is the common enemy: both makers state that the components are sensitive to humidity, and Sika asks that containers be closed tightly right after use.
Handling That Protects the Chemistry
- Open each container as late as possible and reclose it at once, since the makers describe both components as sensitive to moisture.
- Check the polyol for crystals after cold storage, and warm it as the maker describes. Sika allows heating the affected component to 70 °C at most, and Renishaw describes 2 hours at 70 °C followed by a stabilizing period at 40 °C.
- Shake component B before weighing, and weigh with an allowance for the residue that stays in the upper cup.
- Degas each component on its own for 10 minutes before mixing, then mix under vacuum for the time the sheet prints, which is 1 minute or more for PX331 and about 45 seconds for PX 223 HT.
Choosing Between the Four Grades for a Housing, a Hot Part or a Snap Fit
The sheets let a buyer sort the four grades by the job, as long as the sorting stays inside what they print. A housing that needs a flame rating narrows the field at once: PX331 and 8263 both state UL 94 V-0, the first at 3 mm and the second without a thickness on its sheet. Heat narrows it in another direction. PX 223 HT lists a glass transition of 120 °C (248 °F) and 6230 lists 98 °C (208 °F) heat deflection under 1.80 MPa, against 90 °C (194 °F) for PX331 and 80 °C (176 °F) for 8263.
A part with a snap hook or a thin latch looks at elongation. The 4 percent of PX331 leaves little room to flex, while 6230 and 8263 print 14 and 15 percent, and PX 223 HT prints 11 percent. Elongation at break is a tensile figure from one test bar, so a latch geometry still needs a trial part, but the ranking is a fair starting point.
Oven time differs too, and the schedule shows it. The table below turns the post-cure lines of Table 2 into oven hours per copy, counting the demold soak and the post-cure together.
| Grade | Soak in the mold at 70 °C | Post-cure on the sheet | Oven hours per copy, about |
|---|---|---|---|
| PX331 | 45 to 75 min | 1 h at 70 °C plus 16 h at 80 °C | 18 |
| PX 223 HT | 45 to 70 min | 1 h at 70 °C, 1 h at 100 °C, 12 h at 110 °C | 15 |
| 6230 | 25 to 60 min | none | 0.5 to 1 |
| 8263 | 60 min | none | 1 |
The oven hours are a sum of the sheet’s own figures, not a figure the makers state. They show why a grade without post-cure suits a short calendar, and why a grade with a long post-cure is cast in groups, one oven load per day, with the copies held on conformers overnight. A buyer who needs the datasheet values and the shortest calendar asks for both in the same sentence, and the casting house says which grade honors both.
Datasheet Gaps Between a Printed Grade and a Delivered Part
Comparing grades from different makers runs into method differences that the sheets do not reconcile. The glass transition of PX331 is listed under ISO 11359, that of 6230 under a thermomechanical analysis method, and that of PX 223 HT under ASTM E1545. ISO 11359-2 describes thermomechanical analysis for the coefficient of linear expansion and the glass transition, so the first and second are related, while the third is a different standard that may read a few degrees apart on the same material.
The thermal figures name their methods as follows:
- PX331 gives heat deflection under ISO 75A and a glass transition under ISO 11359, with no expansion figure.
- PX 223 HT gives a glass transition by TMA under ASTM E1545 and an expansion coefficient under ISO 11359-2 of 115 ppm/°C (64 ppm/°F), with no heat deflection figure.
- 6230 gives heat deflection under ISO 75 at 1.80 MPa on a 110 × 12.7 × 6.4 mm bar, a TMA glass transition and an expansion figure under JIS K 6911.
- 8263 gives heat deflection on the same bar size without naming the method, and no glass transition.
Heat figures are comparable only inside a maker’s own sheets, and a few more gaps matter in practice:
- No sheet states a value for creep, fatigue or long-term heat aging.
- Impact resistance appears as Charpy, Izod or ASTM D256, so a ranking needs the test method printed beside every value.
- The sheets quote typical values from laboratory specimens, and Sika’s own text adds that measured data may vary with circumstances beyond its control.
- Renishaw’s text says users should carry out sufficient tests to establish suitability for the intended application.
The honest read of an ABS-like datasheet is that it ranks grades inside one maker’s range well and compares across makers poorly. When a drawing calls for a heat or impact figure, the buyer asks the casting house which grade it uses and for the conditions under which the figure was measured. A first article cast in that grade, post-cured the way the sheet describes, settles the question faster than any comparison of sheets.
Whether a given grade keeps the printed Shore D after 1,000 hours near its heat deflection temperature is not something any of these sheets answers. That figure comes from a test on the actual part, run before the order grows past the first tool, and it is the number the datasheet cannot supply.
Parts that need this material in a run of dozens to a few hundred copies are a fit for low-volume vacuum casting, and the same ABS-like resins carry a program into bridge production until a hard tool is cut.
Sources and Further Reading
- Sika, SikaBiresin PX331, product data sheet, version 01.01, 08-2026
- Sika, PX 223 HT, technical data sheet, version 01, February 2021
- Renishaw, Data sheet: vacuum casting resin 6230, issued 09.2015
- Renishaw, Data sheet: vacuum casting resin 8263, issued 05.2015
- Renishaw, Brochure: vacuum casting systems, issued 10.2017
- Estonian Centre for Standardisation and Accreditation, ISO 11359-2:2021, plastics, thermomechanical analysis, part 2, scope
- Estonian Centre for Standardisation and Accreditation, EVS-EN ISO 75-2:2013, plastics, determination of temperature of deflection under load, part 2, scope
- Estonian Centre for Standardisation and Accreditation, EVS-EN 60695-11-10:2013, test flames, 50 W horizontal and vertical flame test methods, scope