Heat deflection temperature ranks materials under one loaded test and does not set a service ceiling, so it is read together with post-cure and part geometry.

Plain rectangular cast polyurethane test bars in black, grey and white, unmarked.

SikaBiresin PX205 comes out of its 70 °C (158 °F) mold at a temperature 15 °C above the 55 °C (131 °F) heat deflection temperature printed on its own data sheet. The sheet’s post-cure of 16 hours at 80 °C (176 °F) is 25 °C above it. A reader who takes the number as a ceiling for the part would expect a deformed casting at every step, and the reason the parts survive is that the number was never a ceiling.

Heat deflection temperature, abbreviated HDT, is one of the most quoted and most misread values on a casting sheet. This piece reads the two standards behind it, lays the three ISO loading methods in a table, collects what the casting makers print, and shows how the number interacts with the oven temperatures of the process.

Heat Deflection as One Loaded Bar Test

The test bends a bar under a fixed load while the temperature climbs, and it records the temperature at which the bar has deflected by a set amount. ISO 75-1 describes the general method for determining the temperature of deflection under load, with flexural stress applied in three-point loading. ASTM D648 describes the same idea as the temperature at which an arbitrary deformation occurs when specimens are subjected to an arbitrary set of testing conditions, which is an unusually frank way for a standard to introduce itself.

Both texts put limits around the result. ISO 75-1 says the methods suit assessing the relative behavior of different materials at elevated temperature under load at a specified rate of temperature increase. The standard adds that the results do not necessarily represent maximum applicable temperatures, since time, loading conditions and surface stress in service can differ from the test, and it states that the data are not intended to predict end-use performance or serve design analysis.

HDT ranks materials under one defined test. It does not say how hot a part can run, because the test fixes a load, a heating rate and a deflection that a real part rarely matches.

The standard goes further on comparability. ISO 75-1 says true comparability of data can only be achieved for materials with the same room-temperature flexural modulus, and ISO 75-2 repeats the point, calling the method suitable only for comparing materials with similar room-temperature elastic properties. For casting resins, whose flexural moduli on the sheets run from 500 MPa (73 ksi) for PX205 to 3,700 MPa (537 ksi) for PX331, that caveat applies directly to the way the grades are ranked.

The Three ISO 75 Methods in One Table

ISO 75-2 specifies three methods that differ in the constant flexural stress applied to the bar. The table sets them beside the ASTM test, as described in the scope text of each standard.

Table 1. Loading methods and scope of the two heat deflection standards
Method Flexural stress Scope text
ISO 75-2 method A 1.80 MPa (261 psi) plastics, including filled plastics and fiber-reinforced plastics with fiber up to 7.5 mm, and ebonite
ISO 75-2 method B 0.45 MPa (65 psi) the same materials
ISO 75-2 method C 8.00 MPa (1,160 psi) the same materials
ASTM D648 set by the standard’s procedure molded and sheet materials 3 mm (0.125 in) or thicker that are rigid or semirigid at normal temperature

ISO 75-1 adds that the test is also known as the heat distortion temperature test, although no official document uses that designation. A sheet that prints HDT without a method letter leaves the reader unable to tell which of the three stresses was applied. Of the casting sheets opened, only some name the method: Sika writes ISO 75A, which is method A at 1.80 MPa, and Renishaw’s 6230 sheet states ISO 75 with a load of 1.80 MPa.

Thickness as a Condition of the Method

ASTM D648 applies to molded and sheet materials available in thicknesses of 3 mm or greater. For thinner sheet, between 1 mm and 3 mm, it allows a composite sample at least 3 mm thick, with the layers cemented at the ends. A thin cast wall therefore has no direct HDT of its own. The number on a sheet describes a bar that is thicker than the wall of many cast parts, and a 1.5 mm housing wall is outside the range where the standard’s single-layer method applies.

Casting Sheets and the Deflection and Glass Transition They Print

Casting makers print heat deflection and glass transition side by side, and the two values answer different questions. The glass transition marks where the cured polymer softens in a thermal analysis scan, while HDT marks where a loaded bar bends by a set amount. Table 2 collects the pairs printed on the sheets opened for these resources and adds a computed gap between them.

Table 2. Heat deflection and glass transition as printed, with the computed gap between them
Resin Heat deflection Glass transition Gap, Tg minus HDT Cure behind the values
SikaBiresin PX205 55 °C (131 °F), ISO 75A 90 °C (194 °F), ISO 11359 35 °C 16 h at 80 °C
SikaBiresin PX331 90 °C (194 °F), ISO 75A 100 °C (212 °F), ISO 11359 10 °C 1 h at 70 °C plus 16 h at 80 °C
SikaBiresin PX522 85 °C (185 °F), ISO 75A 95 °C (203 °F), ISO 11359 10 °C 4 h at 80 °C plus 16 h at 100 °C
SikaBiresin PX523 85 °C (185 °F), ISO 75A 100 °C (212 °F), ISO 11359 15 °C 16 h at 100 °C
Renishaw 6230 98 °C (208 °F), ISO 75 at 1.80 MPa 115 °C (239 °F), TMA 17 °C none
Renishaw 8263 80 °C (176 °F), method not named not measured not available none
Sika PX 223 HT not stated 120 °C (248 °F), TMA ASTM E1545 not available 1 h at 70 °C, 1 h at 100 °C, 12 h at 110 °C

The gap column shows the spread. A stiff resin such as PX331 has its heat deflection within 10 °C of its glass transition, while soft PX205, with a flexural modulus of 500 MPa, loses its stiffness 35 °C before its glass transition. The spread agrees with ISO 75-2’s remark that the result depends on room-temperature modulus, though the sheets alone cannot separate that effect from the cure each grade received.

Another detail needs care. The two columns follow different methods, so a comparison works within a row and not between makers. Sika’s glass transition on PX331 is listed under ISO 11359, and Renishaw’s on 6230 under a thermomechanical analysis method, which ISO 11359-2:2021 describes as the way to determine the coefficient of linear thermal expansion and the glass transition by TMA.

Two Different Ways to Find a Softening Point

The glass transition on a casting sheet does not come from a bending test. ISO 11359-2:2021 specifies thermodilatometry, a method that follows the length of a small solid specimen as it is heated by thermomechanical analysis, and it states that the same method also gives the glass transition. The specimen is not loaded in bending, and the heating regime differs from the 75 standards, so the two softening points need not agree. ASTM E1545, which PX 223 HT names for its 120 °C (248 °F) figure, is a third document, and no sheet reconciles it with ISO 11359.

Subtracting one number from the other and calling the result a margin is therefore a mistake. The gap column in Table 2 only describes the printed pairs and nothing more, and the pairs come from different test setups.

How the Oven Temperatures Meet the HDT

The figures in the table meet the oven temperatures of the process, and the arithmetic is worth doing once. A casting made in a 70 °C mold leaves the oven at roughly that temperature, so a part is at 70 °C when it comes out. Table 3 compares each grade’s printed heat deflection with the mold temperature and the post-cure the sheet asks for.

Table 3. Printed heat deflection set against the process temperatures on the same sheet
Resin HDT Demold temperature Peak post-cure temperature HDT minus peak post-cure
PX205 55 °C 70 °C 80 °C 25 °C below
PX331 90 °C 70 °C 80 °C 10 °C above
PX522 85 °C 70 °C 100 °C 15 °C below
PX523 85 °C 70 °C 100 °C 15 °C below
6230 98 °C 70 °C no post-cure not applicable

Three of the five sheets in the table ask for a post-cure above the grade’s HDT. That sounds alarming and is not, because the HDT test loads the bar at 1.80 MPa (261 psi), a stress that a lightly supported part in an oven does not carry. A part resting on a flat tray in a 100 °C oven sees only its own weight. The risk is of slow sag or bow, and the sheets name the remedy: Sika recommends a conformer, a fixture shaped like the part, depending on its geometry and weight, and the PX 223 HT sheet says the part has to be supported in the oven so that it keeps its shape.

Two sentences summarize the interaction:

  • A grade whose HDT lies below the post-cure temperature needs the part supported during post-cure, whatever the part’s shape.
  • A grade whose HDT lies above its post-cure temperature, like PX331 at 90 °C against 80 °C, keeps a margin, and the sheet does not turn that margin into a promise about thin walls.

Test Bars Behind the Printed Number

Renishaw’s 6230 sheet states its HDT on a test piece of 110 mm × 12.7 mm × 6.4 mm (4.33 × 0.50 × 0.25 in), and the 8263 sheet names the same bar. Sika’s sheets print ISO 75A figures and name no bar size at all, so the two makers’ numbers rest on specimens that a reader cannot compare.

A buyer who relies on the figure asks the maker how the bar was made and how thick it was. For a part with walls of 2 mm, the HDT printed on the sheet is a ranking number, and a deflection check on the real part under a real load is the only direct answer.

Staged Post-Cures and the Glass Transition

PX 223 HT shows a different way of working around the numbers. Its post-cure rises in three steps: 1 hour at 70 °C (158 °F), 1 hour at 100 °C (212 °F) and 12 hours at 110 °C (230 °F), against a glass transition of 120 °C. Each step stays below the transition that the finished material reaches, and the ramp does not start at the final temperature.

That reading is the writer’s, since the sheet does not say why the post-cure is staged. It is consistent with the sheet’s other instruction, that the part is supported in the oven so it keeps its shape.

Delivery quality follows from the same schedule. A part with the first step only has not reached the Tg printed on the sheet, and its heat resistance is lower than the printed figure suggests. The cure record, hours at each temperature, is the evidence that the part matches the sheet.

The heat resistance printed for a casting resin belongs to a part that has had the sheet’s full post-cure. A part with less carries less.

Choosing a Resin Against a Service Temperature

A working method for a buyer uses the printed numbers in a defined order, and the order keeps the standard’s own limits in view:

  • Fix the highest temperature the part sees in service, and the load it carries at that temperature.
  • Keep that temperature well below the printed HDT of the grade, since the standard says HDT is not a maximum applicable temperature.
  • Check the post-cure the sheet attaches to the HDT, and plan the same cure for the delivered part.
  • Ask whether the wall thickness of the part is within the range the standard covers, which starts at 3 mm for ASTM D648.
  • Soak a first article at the service temperature under its real load, and measure the shape afterward.

Each step maps to a line in the standards or on the sheets: the first to the loading in ISO 75-2, the second to ISO 75-1’s warning about maximum temperature, the third to the footnotes behind each printed value, the fourth to the 3 mm lower bound in ASTM D648, and the fifth to nothing at all, which is why it comes last and carries the decision. None of those steps uses a number the sheets omit. A part for a 60 °C enclosure, for instance, sits 25 °C below the 85 °C of PX522, and the questions that remain are the load, the wall thickness and the post-cure, in that order. For a part that sees 85 °C, the printed HDT of every grade except PX331 and 6230 is at or below the service temperature, and those two sit only 5 °C and 13 °C above it, and the choice moves to a different resin family or to a part redesign that spreads the load.

Soaking a First Article at Service Temperature

A soak is the simplest direct answer to a heat question. The first article goes into an oven at the service temperature for a set time with its working load or a stand-in for it, and the dimensions that matter are measured before and after. A bow, a sag or a closing of a snap fit shows at once. The test costs hours and uses equipment every casting room already owns, since the post-cure oven runs the same temperatures.

The record that makes the soak useful is short. It names the grade, the post-cure the part received, the temperature, the time, the support used and the measured change. With that record, a later batch cast from the same grade and cure is compared to it directly, which is exactly the kind of control the standards leave to the buyer.

Limits Written Into the Deflection Tests

The standards themselves list their gaps. ISO 75-2 states that the methods give better reproducibility with amorphous plastics than with semi-crystalline ones, and that some materials may need annealing of the test specimens to give reliable results. Annealing generally raises the temperature of deflection under load. A cast thermoset that has had its post-cure behaves in the same way as an annealed bar, and the sheets show it: the values printed for PX331 rest on 17 hours of oven time at 70 °C to 80 °C, and a part delivered straight from the mold has not had it.

ASTM D648 adds that its result applies to an arbitrary set of test conditions, so a figure from one machine and loading cannot stand for another. Neither document sets a pass limit, because neither is a specification.

For a drawing, the usable statement names the grade, the ISO 75 method and stress, the post-cure of the test bar and the minimum temperature the part has to reach in service. The first article then carries the same post-cure, and a heat soak at the service temperature confirms the part holds its shape. Programs running dozens to a few hundred parts in low-volume vacuum casting record the post-cure on each batch, and the same record carries into bridge production when the tool changes.

Sources and Further Reading

Send the Drawing of Your Cast Part

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Vacuum Casting chosen.

Request a Quote